Ironmaking and Steelmaking
Next Article in Special Issue
Annealing Response of a Cold-Rolled Binary Al–10Mg Alloy
Previous Article in Journal
Microstructural Characterization and Formation Mechanism of Nitrided Layers on Aluminum Substrates by Thermal Plasma Nitriding
Previous Article in Special Issue
Effect of Eutectic Mg2Si Phase Modification on the Mechanical Properties of Al-8Zn-6Si-4Mg-2Cu Cast Alloy
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Influences of Cu Content on the Microstructure and Strengthening Mechanisms of Al-Mg-Si-xCu Alloys

1
Hunan Provincial Key Defense Laboratory of High Temperature Wear-resisting Materials and Preparation Technology, Hunan University of Science and Technology, Xiangtan 411201, China
2
School of Materials Science and Engineering, Central South University, Changsha 410083, China
*
Authors to whom correspondence should be addressed.
Metals 2019, 9(5), 524; https://doi.org/10.3390/met9050524
Submission received: 11 April 2019 / Revised: 28 April 2019 / Accepted: 3 May 2019 / Published: 7 May 2019
(This article belongs to the Special Issue Phase Transformations in Aluminium Alloys)

Abstract

:
The effects of the Cu content on the microstructure and strengthening mechanisms of the Al-Mg-Si-xCu alloys were systematically investigated using scanning electron microscopy (SEM), electron probe microanalysis (EPMA), transmission electron microscopy (TEM), and mechanical tensile tests. The results show that, the strengthening mechanisms change with the Cu content. For as-quenched alloys, solution strengthening (σSS) is predominant when the Cu content ≥2.5 wt.%, and of equivalent importance as grain size strengthening (σH-P) when the Cu content ≤1.0 wt.%. With respect to peak-aged alloys, precipitation strengthening (σppt) is predominant when the Cu content ≥2.5 wt.%, but σSS becomes predominant when the Cu content is 4.5 wt.%. As the Cu content increases from 0.5 to 4.5 wt.%, the main type of precipitates in alloy tends to change from a β″ phase to Q′ phase, and then to a θ′ phase. Among the three types of precipitates, θ′-precipitate causes the largest increase in yield strength (σ0.2) and the largest decrease rate in elongation. β″-precipitate leads to the smallest increase in σ0.2 and the smallest decrease rate in elongation. The increase of Cu content reduces Si solubility in the Al matrix and thus decreases the nucleation rate of β″ phase during subsequent aging.

Graphical Abstract

1. Introduction

Al-Mg-Si-xCu alloys have been widely used in the fields of aviation, rail transportation, and the automobile industry, due to the combination of good formability and excellent corrosion resistance [1,2]; however, the relatively low strength has restricted their applications, due to the increasing requirements for larger, faster vehicles. Thus, it is necessary to develop Al-Mg-Si-xCu alloys with better mechanical properties [3,4].
Cu is known to have a significant strengthening effect on Al-Mg-Si-Cu alloys [5]. Many studies [6,7] show that the strength of such an alloy can be enhanced by Cu additions as low as 0.1 wt.%. Jin et al. [5] indicated that additions of 0.3 wt.% Cu increased the tensile strength of Al-Mg-Si-Cu alloys from approximately 390 to 430 MPa. Shabestari et al. [8] found that an increase in Cu content from 0.2 to 1.5 wt.% could lead to an increase of around 25% in the tensile strength of such alloys. Zheng et al. [9] discovered that, when the addition of Cu increased to 4.0 wt.%, the strength of the alloy was increased by more than 37.5%. On account of the increasing demand for high-strength alloys, the recent interest in Al-Mg-Si-Cu alloys has been switched to alloys with a wider range of Cu contents; however, as research continues, issues concerning the Cu effect on the microstructure and mechanical properties of Al-Mg-Si-Cu alloys have gradually emerged, as discussed below.
(i) In many research projects [10,11,12], it has been found that, with the increase in Cu content, the tensile strength of the alloy increases, while the ductility of the alloy decreases: However, in some studies, it has been shown that Cu additions can increase the strength of an alloy without an accompanying loss of ductility. Jin et al. [5] and Zhong et al. [13] even found that 0.3 and 0.6 wt.% additions of Cu increase both the strength and elongation of such an alloy. Besides, some researchers found that the strength of the alloys does not always monotonically increase with Cu content. For instance, Lu et al. [14] found that the tensile strength of such an alloy decreases when the Cu content increases from 1.48 to 1.86 wt.%.
(ii) It is known that, Cu additions can produce grain size strengthening (σH-P), solid solution strengthening (σSS), and precipitation strengthening (σppt) effects on Al-Mg-Si-Cu alloys, but it remains unclear which effect is predominant, especially in alloys with different Cu contents. Watanabe et al. [15] and Sauvage et al. [16] investigated the strengthening behavior of Al-Mg-Si-Cu alloys with 0.2–0.7 Cu wt.% contents, and attributed the strengthening effect of Cu to the significant grain refinement therein. However, Salleh et al. [17] stated that Cu addition has no significant effect on grain refinement, and indicated that σppt plays a major role in the increase of hardness and tensile strength. Although many studies [11] support the view of Salleh et al., others [18] have stated that the significant increase in maximum hardness during ageing, with the increase in Cu content, is mainly the results of σSS.
(iii) It is known that different types of precipitates (e.g., β″ [15], Q′ (Al3.8Mg8.6Si7Cu1) [5,16], σ (Al5Cu6Mg2) [19], θ′(Al2Cu) [9], etc.) might be present, and often coexist, in Al-Mg-Si-Cu alloys during artificial aging, but their strengthening effects on such alloys were still widely debated. Esmaeili et al. [20] found that both β″ and Q′ precipitates occurred in the peak-aged alloy, but only the β″ precipitate was the main cause of age-hardening. Wang et al. [18], and Lu et al. [14], support Esmaeili et al. Miao et al. [21], and Saito et al. [7] stated that the Q′ precipitates were mostly formed in over-aged conditions rather than peak-aged conditions: However, some other studies find that both β″ and Q′ precipitates contributed to the strength increase of the alloy. Moreover, Jin et al. [5] and Farkoosh et al. [10] found that the Q′ precipitate plays the major role in improving the age-hardening of alloys with Cu addition.
In short, quaternary Al-Mg-Si-Cu alloys, straddling the compositions of 2xxx (Al-Cu(-Mg)) and 6xxx (Al-Mg-Si) alloy, are more widely used in applications, due to their excellent comprehensive performance. The Cu content is known to have a pronounced effect on both microstructure and the properties of Al-Mg-Si-Cu alloys, but details thereof remain unknown. Therefore, uncovering the effect of Cu content on the microstructure and strengthening mechanisms of Al-Mg-Si-Cu alloys is important for alloy designers. Here, Al-Mg-Si-Cu alloys with four different Cu contents (0.5 wt.%, 1.0 wt.%, 2.5 wt.%, and 4.5 wt.%) were designed, and SEM, EPMA, TEM, and mechanical tensile tests were used to study the effects of the Cu content on the microstructure, aging precipitation, and mechanical properties of the Al-Mg-Si-Cu alloys.

2. Experimental Methods

2.1. Materials

Four Al-Mg-Si-Cu alloys with different Cu contents were produced using high purity aluminium (>99.97 wt.%), oxygen-free copper (>99.95 wt.%), an Al-20% Si master alloy, industrially-pure magnesium (>98 wt.%) and an Al-5% Ti-1% B grain refiner. The specific compositions of these alloys (Alloy 1, 2, 3, and 4) are listed in Table 1.
To acquire a homogeneous microstructure, the alloy ingots (φ 400 mm × L 200 mm) were subjected to homogenization annealing (Alloy 1 and Alloy 2 were homogenized at 560 °C for 12 h, and Alloy 3 and 4 were homogenized at 520 °C for 12 h) in an air furnace. Then, the ingots were extruded into a bar with a diameter of 10 mm at 440 °C and cut into 10 mm long cylindrical samples. Post solution heat treatment of the alloys was conducted in an SG-12-10 salt-bath furnace at 520 °C for 1 h, followed by water quenching, and then, an artificial aging treatment was undertaken at 165 °C for different times immediately after quenching with a room-temperature storage time less than 30 s.

2.2. Performance Test

The mechanical tensile tests were performed on a DDL 100 electronic universal testing machine (Changchun Research Institute for Mechanical Science Ltd., Changchun, China) with a tensile speed of 2 mm/min. The size of the tensile samples is illustrated in Figure 1. The hardness testing of each alloy sample was performed using a load of 30 N and a dwell time of 15 s.

2.3. Microstructure Analysis

Metallographic specimens were prepared using a standard procedure and were etched in a solution containing HF (2 mL), HCl (3 mL), HNO3 (5 mL), and H2O (200 mL). The grain size was determined by a line intersection method, according to ASTM E112-96, which involves an actual count of the number of grains intercepted by a test line. For each testing sample, at least 200 grains were considered.
The distribution characteristics of second-phase particles were obtained by the use of a JXA-8230 electron probe microanalyzer (EPMA, JEOL Ltd., Tokyo, Japan). The wavelength dispersion spectrometer (WDS, JEOL Ltd., Tokyo, Japan) was used to quantify the composition of the second-phase particles in the alloy and to observe the distribution of the main elements of the alloy.
The TEM, high-resolution transmission electron microscopy (HRTEM), and high-angle-annular-dark-field scanning transmission electron microscopy (HAADF-STEM) images were carried out on a Tecnai G2 F20 (FEI Ltd., Hillsboro, OR, USA) and Titan G2 60-300 TEM (FEI Ltd., Hillsboro, OR, USA), and the accelerating voltage of both the instruments was 200 kV. Thin foils for the TEM analyse were prepared in a twin-jet electro-polishing unit using a solution of nitric acid: methanol (1:3 by volume) at −25 °C, 20 V, and a current of about 80 mA.

3. Results

3.1. Effect of Cu Content on the Metallographic Structures of the Alloys

Figure 2 shows the metallographic structures of the four alloy samples in both as-extruded, and as-quenched, states. The average grain size (AGZ) and grain aspect ratio (GAR) of these alloys were calculated, and the results are listed in Table 2. In the as-extruded state, the grains of all four alloys were elongated along the extrusion direction (ED), and AGZs were measured to be 765, 538, 475, and 190 µm, respectively. The grains in Alloys 1 and 2 generally take on pancake shapes with GARs of 6.47 and 8.27, respectively, but the grains in Alloys 3 and 4, exhibiting remarkably fibrous characteristics, show apparently larger GARs.
In as-quenched states, the AGZs of all four alloys were measured to be 482, 351, 211, and 108 µm, respectively, which decreased compared with those of the as-extruded alloys. Besides, the AGZs of alloys significantly decrease, while the GARs of alloys increase as the Cu content increases. As seen, compared with Alloy 1, the AGZ of Alloy 4 decreases by 75.2% and its GAR increases by 75.4%. This indicates that the Cu addition plays an important role in both grain refinement and increasing GAR.
Figure 3 shows the {200} pole figures of four as-quenched alloys, respectively. A texture with a pole of high intensity is seen in the center of the {200} pole figure for all four alloys, which implies an evident fiber texture developed on the {200} planes after quenching. Besides, this {200} fiber texture is sharper with the increase of Cu content, which confirms that the recrystallisation is more pronounced in the alloy with a higher Cu content, since the {200} fiber texture is known to be a typical recrystallisation texture in aluminium alloys [22].

3.2. Influence of Cu Content on the Coarse Second-phase of the Alloys

Figure 4 shows the back-scattered electron (BSE) images of the four alloys in both the as-extruded, and as-quenched, states. A large number of coarse second-phase particles, arranged along ED, were observed in all four as-extruded alloys (Figure 4a,c,e,g), and their number increases with the increase of Cu content. After solution heat treatment, the number of coarse second-phase particles decreases, but many of them are still reserved especially for the alloys with high Cu contents (Figure 4h).
Figure 5 and Figure 6 show elemental mapping of as-extruded and as-quenched samples of Alloy 1. There are two types of coarse second-phase particles: Ellipsoidal second-phase particles and white rod-shaped second-phase particles. The grey second-phase particles are rich in Fe, Si, and Mn, but the white ones are mainly rich in Cu and Si. According to the literature, the grey phase is determined to be an Al(Fe,Mn)xSiy phase [23] and the white phase is identified as an AlCuxSiy phase [5], which are the common inclusions in Al-Mg-Si-Cu alloys. As can be also noticed, the number density of Al(Fe, Mn)xSiy particles is significantly larger than that of the AlCuxSiy phase in Alloy 1 in both as-extruded, and as-quenched, states.
By comparing the maximum intensity values (Imax) of each element in the EPMA mapping, the element distribution can be obtained. Among the tested elements, Mg and Si have quite low Imax values in Alloy 1 in both as-extruded and as-quenched states, implying that they are distributed relatively evenly. This is probably due to the high solubility and diffusion coefficient of Mg and Si in Al [24]. Although the Cu content is similar to the contents of Mg and Si in Alloy 1, Imax,Cu is much larger than Imax,Mg and Imax,Si which indicates that the Cu distribution is less uniform. In addition, it is shown that, after solution heat treatment, Imax,Cu, Imax,Mg, and Imax,Si decrease slightly but Imax,Mn and Imax,Fe increase. This means that the elements of Cu, Mg, and Si in the coarse second-phase particles gradually dissolve into the matrix while an enrichment of Mn and Fe elements in the coarse second-phase particles takes place.
Figure 7 and Figure 8 show elemental mappings of as-extruded and as-quenched samples of Alloy 4. Differing from Alloy 1, almost all the coarse second-phase particles display a significant increase in the amount of Cu. The AlCuxSiy phase was transformed into a θ (Al2Cu) phase [25], which was depleted in Si. Imax,Cu and Imax,Mg decrease, while Imax,Fe and Imax,Mn increase after solution heat treatment. In contrast to that of Alloy 1, Imax,Si increases from 11.0% to 57.1%, suggesting that the Si content in the second-phase particles increases after solution heat treatment.

3.3. Influence of the Cu Content on the Mechanical Properties of the Alloys

3.3.1. Age-Hardening Curves

The artificial age-hardening of as-quenched alloys (at 165 °C) was studied in our previous work [4], and here is also shown in Figure 9. It is shown that the hardness of alloys and the peak-aging time increase with the Cu content. After peak aging, the hardness of all four alloys decreases. When the alloys are aged for 14,400 min, the hardness values for Alloys 1, 2, 3, and 4 have decreased by 36, 29, 37, and 85 HV, respectively, relative to their peak-aging hardness values. This indicates that the over-aging softening phenomenon is more obvious in Alloy 4 than in the other three alloys.
Here, we continue our previous work by evaluating the tensile mechanical properties and their relationship with precipitation in alloys with different Cu contents.

3.3.2. Mechanical Properties

Figure 10a shows the tensile curves of the four as-quenched alloys. The strengths of Alloys 1–4 are enhanced with increasing Cu content, in particular, the tensile strengths of Alloys 3 and 4 are enhanced by 54.8%, and 104.1%, respectively, compared with that of Alloy 1. The elongations of Alloys 1 and 2 are 29.7%, and 28.1% respectively, illustrating that the decrease in elongation is quite limited when the Cu content increases from 0.5% to 1.0%, but when the Cu content increases to 2.5%, the elongation of alloy decreases with the increase of Cu content. The elongations of Alloys 3 and 4 decrease to 20.6%, and 18.5%, respectively. This suggests that the elongations of Alloys 3 and 4 decrease by 30.6%, and 37.7%, respectively, compared to that of Alloy 1.
Figure 10b illustrates the tensile curves of the four alloys in peak-aged state. The strength of all four alloys are enhanced to a certain extent compared with those of as-quenched alloys, and are measured to be 261.3, 270.9, 346.2, and 442.5 MPa, respectively. Meanwhile, the elongations of Alloy 1–4 are 19.3%, 17.9%, 11.6%, and 10.0%, respectively. This indicates that the strength of the alloys significantly increases while their elongation decreases when the Cu content increases to 2.5%. Besides, in our study, it shows that either the Cu content or the aging treatment has little influence on the elastic modulus of aluminium alloy, which is in accordance with the results of previous studies [6,7].

3.4. Influence of the Cu Content on the Precipitates of the Alloys

Figure 11 shows TEM and corresponding selected area diffraction pattern (SADP) images of the four alloys in peak-aged state. In all four alloy samples, there are many precipitate particles distributed uniformly in the Al matrix. The shapes of precipitates in Alloys 1 and 2 (Figure 11a,d) are similar and are of acicular or granular form. Among these precipitates, the acicular ones were arranged along the <010>Al directions. In addition, the number density of granular precipitates is larger and the number density of acicular precipitates is smaller than those in Alloy 1. The SADP image of Alloy 1 (Figure 11b,c) shows faint cruciform diffraction spots in the central positions of the (000) and (202)Al spots, but an break can be observed in the middle position of the cruciform diffraction spots for Alloy 2 (Figure 11e,f). This implies that the precipitates in Alloy 1 and 2 may be not the same.
Figure 11g–l illustrates the TEM images and corresponding SADP results for the peak-aged Alloys 3 and 4. In Alloys 3 and 4, the acicular precipitates are replaced by lamellar-shaped ones. Besides, the number of granulate-shaped precipitates decrease compared to that of the other three alloys. The SADP images of Alloy 3 and 4 are similar: Distinct cruciform diffraction spots, due to the precipitates are observed between (000) and (002)Al, (000) and (200)Al, (200)Al and (202)Al, and (002)Al and (202)Al, but the diffraction spots of the precipitates are brighter in Alloy 4, which may be related to its more numerous and thicker lamellar-shaped precipitates, compared with those in Alloy 3.
To further determine the type of precipitate in these alloys, HRTEM and HAADF-STEM were used. Figure 12 shows the HRTEM results for the typical granular-shaped precipitate in the peak-aged Alloy 1. As shown in Figure 12a, this precipitate has a monoclinic structure with lattice parameters of a = 1.51 nm and c = 0.67 nm. According to Figure 12b,c, the orientation relationships of (200)precipitate∥(301)Al and [010] precipitate∥[010]Al can be detected. Therefore, the granular-shaped precipitate is determined to be the β″ phase [4,15].
Figure 13a shows the HRTEM results for the typical acicular precipitates in the peak-aged Alloy 1 which is approximately four Al atom layers in width but over 100 Al atom layers in length. Due to its acicular shape feature, the precipitate usually overlaps with the Al matrix, and it is thus difficult to observe its lattice structure viewed in the edge-on direction [26], but the corresponding FFT (Figure 13b,c) reveals that these precipitates are a β″ phase. Therefore, both the acicular, and granular-shaped, precipitates are of the β″ phase. Their different shapes are only caused by differences in viewing direction, namely, viewed edge-on (acicular) or end-on (granulate shape). Since no other precipitate is observed, the β″phase should be the predominant precipitate in peak-aged Alloy 1.
The β″ phase and Al matrix are known to have a coherent interface with a large interface strain energy, which exerts a favourable effect on the alloy in terms of strength [27]. For the alloys with a low Cu content (Alloy 1), the β″ phase is the main strengthening phase in the peak-aged condition.
Compared with those in Alloy 1, the acicular precipitates in the peak-aged Alloy 2 are relatively coarser. Figure 14a shows the HRTEM image of a typical acicular precipitate particle in Alloy 2 whose width exceeds seven Al atom layers. As shown in Figure 14b,c, this precipitate has the same FFT pattern with that of acicular precipitates in Alloy 1, and is also determined to be the β″ phase.
The HRTEM image and corresponding FFT pattern of the granulated precipitate in the peak-aged Alloy 2 are shown in Figure 15. This precipitate has a polygonal (hexagonal) shape with a typical HCP crystal structure which is different from the shape of the β″phase. Its lattice parameters are determined to be a = 1.032 nm and c = 0.405 nm, besides, its interface is largely parallel to the three crystal faces of the Al matrix, i.e., (501)Al, (103)Al and (506)Al (Figure 15). Moreover, its orientation relationships with the Al matrix are found to be (2110)precipitate∥(501)Al and [0001]precipitate∥[010]Al, i.e., the angle between (2110)precipitate and (200)Al is approximately 9.5°. These results are consistent with previous reports concerning a Q′ phase [4,5,25].
Figure 16 shows the HAADF-STEM image and corresponding energy-dispersive X-ray spectroscopy (EDS) mapping results for the peak-aged Alloy 3, viewed along <010>Al axis. As can be seen, all the granulate-shaped precipitates (shown by broken circles) are enriched in Cu, Mg, and Si, consistent with the ingredients of a Q′ phase; however, the lamellar-shaped precipitates without Mg and Si in Alloy 3 are only enriched in Cu, indicating that these precipitates are not the β″ phase. According to the HRTEM and corresponding FFT images shown in Figure 17, these lamellar precipitates, elongated along {200}Al, exhibit a tetragonal structure with lattice parameters of a = 0.404 nm and c = 0.58 nm. Their orientation relationships with Al matrix are determined to be (200)precipitate∥(200)Al and [010]precipitate∥[010]Al. From the literature [25], it can be concluded that these precipitates are a θ′ phase, and so the predominant precipitates in the peak-aged Alloy 3 are θ′ and Q′ phases.
The HAADF-STEM images of Alloy 4 viewed along <010>Al are shown in Figure 18a: similar to Alloy 3, a large quantity of lamellar precipitates and fine granular precipitates are distributed in Alloy 4. Figure 18b shows the Z-contrast image of the lamellar precipitated phases. This precipitate has an orientation relationship of (200)precipitate∥(200)Al and [010]precipitate∥[010]Al with the matrix. So, this precipitate is considered to be a θ′ phase (see Figure 19). Since this imaging mode is dominated by atomic number, the brightest dots can be identified as atomic columns of Cu (ZCu = 29). Also imaged, but with a lower intensity, are the Al atomic columns (ZAl = 13) within the precipitates and the surrounding matrix. This reveals that the Cu atoms inside these lamellar precipitates have a regular, periodic, distribution.
Figure 18c,d show the HAADF-STEM images of the granulated precipitate. All these precipitates have the same orientation relationship with the Al matrix, i.e., ( 2 1 ¯ 10 ) precipitate∥(501)Al and [0001] precipitate∥[010]Al. Thus, this precipitate is determined to be the Q′ phase. Since Q′ phase is made up of Mg (ZMg = 12), Si (ZSi = 14) and Cu, and Cu has a much larger atomic number than Mg and Si, the brightest dots in the Q′ lattice can also be identified as atomic columns of Cu. As can be seen, the Cu atoms are periodically arranged in this precipitate when viewed along <010>Al.
Figure 19a shows the Z-contrast image of the θ´ phase/Al matrix interface obtained via HAADF-STEM. The lattice constants of the θ´ phase are aθ´ = 0.404 nm, cθ´ = 0.574 nm, and β = 90°. At the Al matrix/θ´ phase interface, (200)Al and (200)θ´ have a favorable, one-to-one corresponding relationship. This indicates that the θ´ phase exhibits a completely coherent interface structure with the matrix. Besides, a change in structure is evident at the coherent interfaces between the θ´ precipitates and the matrix, as additional Cu atoms appear at the interfaces of θ´ precipitates. This agrees with the results reported elsewhere [28,29].
Image intensity profiles taken along (002) planes across the broad interfaces (B1-B2) confirm that the Cu occupancy of the interstitial sites at the interface is almost full for the precipitate in Figure 19b. The interstitial site occupancy was estimated by measuring the interstitial atom column intensities in the experimental HAADF-STEM images and comparing them with intensities for non-interstitial Cu columns. The intensity profiles of the C1-C2 profile illustrates an interstitial site between every two Cu atoms, which is consistent with the θ´ phase atom positioning model proposed by other studies [30,31]. Bourgeois et al. [32] noted that the Cu occupancy of the interstitial sites at the θ´ phase/Al matrix interface change with the thickness of the θ´ phase: Thicker θ´ precipitates exhibit a lower occupancy of interstitial sites at the interface and the interstitial site occupancy rate of Cu is quite low when the thickness of the θ´ phase exceeds 8Cθ´. In the present study, the thickness of the θ´ phase observed in Figure 18 reaches 12.5Cθ´, but the interstitial sites at the interface are still fully occupied by Cu atoms. This is probably due to the different Mg contents in alloys between the present study and Bourgeois et al. [32]. The materials studied by Bourgeois et al. are Al-Cu-Si ternary alloys in which the Cu content was similar to that of Alloy 4 but did not contain Mg. It is known that, the atom radii of Al, Mg, Si, and Cu are 0.143, 0.160, 0.138, and 0.128 nm [33], respectively. The greater atom radii of Mg might play a role in balancing the negative strain produced by the occupied Cu atoms at the interface which increases the interstitial site occupancy rate of Cu.
Figure 20 illustrates the HRTEM image of the granulated precipitates in Alloy 4. According to the lattice measurement and the FFT analysis, it is confirmed that these precipitates are of the Q′ phase.
According to the above analyses, Alloy 4 has the same types of precipitates with alloys which are θ′ and Q′ phases; however, the θ′ phase is dominant in Alloy 4, and the number and size of Q′ phase particles are also smaller than those of Alloy 3.

4. Discussion

4.1. Influence of Cu Content on Alloy Microstructure

4.1.1. Coarse Second-Phase Particles

In Alloy 1, the coarse second-phase particles include the Cu-depleted Al(Fe,Mn)xSiy phase and Cu-riched AlCuxSiy phase. With increasing Cu content, the amount of Cu in the coarse second-phase particles gradually increases. When the Cu content increases to 4.5 wt.% (Alloy 4), almost all the coarse second-phases show some certain enrichment of Cu and the AlCuxSiy phase in Alloy 1 as it transforms into a θ-phase.
As Alloy 1 has a low Cu content (0.5 wt.%), its element distribution changes during solution heat treatment, which is similar to that of Al-Mg-Si alloy in which Mg and Si in the coarse second-phase have been sufficiently dissolved. This is consistent with our observation showing that Mg and Si elements are distributed more uniformly and Imax,Mg and Imax,Si decrease significantly after solution heat treatment. Cu also has a higher solubility in the Al matrix at elevated temperatures, therefore, the Cu element in the coarse second-phase particle gradually dissolves into the Al matrix during solution heat treatment, causing a decrease in Imax,Cu, while, Mn and Fe have limited solubilities in Al, both at room temperature and high temperature, different from Cu, Mg, and Si. Therefore, after solution heat treatment, the Mn and Fe elements still remain in the coarse second-phase, but, since other elements (e.g., Cu, Mg, and Si) dissolve back into the Al matrix, the relative concentrations of Mn and Fe in the coarse second-phase particle increase which leads to an increase in Imax,Mn and Imax,Fe (Figure 5 and Figure 6).
Similar to Alloy 1, the Cu and Mg in the second-phase of Alloy 4 gradually dissolve, and Mn and Fe remain in the coarse second-phase particle during solution heat treatment, but, because Alloy 4 has a much higher Cu content (4.5 wt.%) than that in Alloy 1, the surplus Cu atoms remain in the coarse second-phases, inducing Alloy 4 to have a larger number of coarse second-phase particles after solution heat treatment (Figure 21). Besides, different from Alloy 1, Imax,Si increases from 11.0% for the as-extruded Alloy 4 to 57.1% for as-quenched Alloy 4, which indicates that Si content in second-phase particles after solution heat treatment increases significantly. It should be noted that the difference in the chemical compositions between Alloy 1 and Alloy 4 lies only in the Cu content; however, the Si content in second-phase particles of alloy 4 is higher than that in Alloy 1, especially under the solution heat treatment state. This indicates that a significant increase of the Cu content would decrease Si solubility in Al, contributing to the Si element being preserved in the coarse second-phase particle.

4.1.2. Grain Size

The AGZs of alloy significantly decrease as the Cu content increases, especially for the as-quenched alloys. The Cu content of Alloy 2 is twice that of Alloy 1, and its AGZ in as-quenched state decreases by only 27.1%, compared with as-quenched Alloy 1. The Cu content of Alloy 4 is eight times larger than that of Alloy 1, but its AGZ significantly decreases by 76.1% compared with Alloy 1. This indicates that, when the content of Cu is between 0.5 wt.% and 4.5 wt.%, the grain refinement effect is gradually enhanced with the increase of Cu content.
In Salleh et al. [17] and Zeren et al.’s [11] work on as-cast Al-Mg-Si-Cu alloys, it is shown that the effect of Cu addition on grain refinement is small. This indicates that Cu addition has no significant effect on either growth restriction or enhancing nucleation during α(Al) solidification. In the studies on hot-worked and as-quenched alloys, Cu addition always shows a strong grain-refinement effect. This agrees with our observation, which is probably due to the particle-stimulated nucleation of recrystallisation (PSN) caused by Cu addition [34,35,36]. As shown in Figure 4, the coarse second-phase particles increase with the increase in Cu content. On the one hand, during hot working, these coarse second-phase particles would produce a strong local strain field, which induces dynamic recrystallisation. On the other hand, during solution heat treatment, these coarse second-phase particles can also act as nucleation sites for the recrystallized grains, finally refining the grain sizes. Therefore, Cu addition causes the decreases in grain size of alloys in both hot-worked, and as-quenched, states. This pronounced PSN effect of coarse second-phase particles on Al alloys is consistent with results from Chakrabarti et al. [37], which shows that the increase in amount of coarse θ-phase particles leads to an increase in recrystallisation nucleation of alloys and grain size refinement. Besides, these coarse second-phase particles can also exert a pinning force on the grain boundaries, and thus limit the grain growth and refine the grain size.

4.1.3. Precipitates

With the increase in Cu content, the main precipitates of the peak-aged alloys change from an acicular β″ phase in 0.5 wt.% Cu alloy (Figure 21a) to an acicular β″ phase and granulated Q′ phase in 1.0 wt.% Cu alloy (Figure 21b), a granulated Q′ phase and lamellar θ′ phase in 2.5 wt.% Cu alloy (Figure 21c), and a lamellar θ′ phase with a small amount of Q′ phase in 4.5 wt.% Cu alloy (Figure 21d).
In Al-Mg-Si-Cu alloys, with a Cu content less than or equal to 1.0 wt.%, β″ precipitates are observed and the amount thereof decreases with the increase of Cu content, owing to the formation of Q′ precipitates. The Q′ precipitate is found in Alloys 2, 3, and 4, and its number density decreases with the increase of Cu content. This is probably attributed to the precipitation of lamellar θ′-phase.
It is known that the β″ phase is the main strengthening phase in Al-Mg-Si alloys [38]. At the initial aging stage of β″ precipitate formation, Mg and Si atomic clusters are formed almost simultaneously, but Mg atomic clusters gradually dissolve into the Si atomic clusters during subsequent aging [39,40], therefore, the Si atomic cluster should be the nucleus for the β″ precipitate. As shown in Figure 7, the increase of Cu content could reduce the Si solubility in the Al matrix. Since Alloy 2 has a higher Cu content than that of Alloy 1, the concentration of Si in Alloy 2 should be lower than that in Alloy 1, which suppresses nucleation of β″precipitates and finally leads to the relatively lower number density of β″ precipitates. Besides, in Al-Mg-Si alloys with Mg/Si < 1 (in wt.% terms), it is usually observed that Si-particles form after aging because of the excess of Si [24], but in Alloys 1–4 in which Mg/Si is equal to 0.84, Si-particles are not seen. This could be also due to the decrease in Si solubility in Al, caused by the addition of Cu, since it suppresses the dissolution of Si atoms in the Al matrix during solution heat treatment and thus reduces the supersaturation of Si during aging.
Due to the increase in Cu content in Alloy 2, the major strengthening phase changes to the Q′ phase [37,41,42]. Previous studies have shown that, at a low Cu content (≤1.0 wt.%), the Q′ phase only precipitates in alloy with a small Mg/Si ratio, which usually coexists with β″ phase. Perovic [43] and Chakrabarti et al. [37] found that, when Mg/Si < 1.73, the Q′ phase and β″ phase are the main strengthening phases in the peak-aged Al-Mg-Si-Cu alloy with 1.0 wt.% Cu content. This is consistent with our observation in Alloy 2. For a high Cu content (≥2.0 wt.%), the formation of Q′ phase depends on Cu/Mg ratio of alloy which decreases with the increase of Cu content. This is also found in Alloys 3 and 4 where the Q′ precipitates continue decreasing in amount when the Cu content increases from 1.0 to 4.5 wt.%. In many studies [37,44] of Al-Mg-Si-Cu alloys with Cu contents ranging from 0.1 to 1.0 wt.%, some other types of precipitates (e.g., U1, U2, etc.) were observed. Saito et al. [7] indicated that U1- and U2-precipitates were mainly formed in the over-aging stage. This is consistent with our observation showing that these types of precipitates are not present in peak-aged alloys.
The θ′ phase usually forms in Al alloys with a relatively high Cu content [45,46]. Liu et al. [47] found that the formation of a θ′ phase depends on both the Mg content and Cu/Mg ratio. When the Mg content is less than 1.0 wt.% and Cu/Mg ratio is greater than 2.6, the θ′ phase forms, otherwise, an S phase will form. In both Alloys 3 and 4, the Mg content is equal to 0.42 wt.%, and their Cu/Mg ratios are calculated to be 5.95, and 10.71, respectively, which are much larger than 2.6. Therefore, the θ′ phase precipitates in the alloy and S-phase is not observed. Since both Q′ and θ′ phases contain Cu, the formation of a θ′ phase will significantly reduce the extent of supersaturation of the Cu in solid solution and thus suppress the precipitation of the Q′ phase, therefore, with the increasing formation of θ′ precipitates in Alloy 4, its number density of Q′ precipitates apparently decreases compared to Alloy 3.

4.2. Influence of Cu Content on Alloy Strengthening Mechanisms

4.2.1. Strength

For the as-quenched alloys, the influence of Cu content on the strength of alloy is mainly affected by σH-P and σSS, since the precipitation has not yet taken place. Assuming that different strengthening mechanisms act independently and can be taken into account as being additive, the influence of Cu content on the mechanical properties Al-Mg-Si-Cu alloy can be expressed as follows [48]:
σ0.2,Q = σH-P + σSS
where σ0.2,Q is the yield strength of as-quenched alloy.
The σH-P is generally described by the Hall-Petch equation [49]:
σH-P = σ0 + Kd−1/2
where σ0 is the yield strength of single crystal, K is a parameter related to grain size that describes the relative strengthening contribution of grain boundaries, and d refers to AGZ.
It has been shown that, for Al alloys with AGZ > 50 µm, K is a constant which generally lies within the range 0.17 to 0.22 [48,50,51]. The AGZs of Alloys 1–4 are 482, 351, 211, and 108 µm, respectively. Even using the maximum value of K (0.22), the σH-P value of four alloys are only 10.0, 11.8, 15.2, and 21.2 MPa, respectively. Then, the increase of σ0.2 caused by σSS for Alloys 2–4 compared with Alloy 1 can be calculated to be 5.2, 61.3, and 146.6 MPa, respectively. This indicates that the increase of σ0.2 for as-quenched alloys is mainly attributed to the σSS at high Cu contents (≥2.5 wt.%). It is known that Cu atoms in Al-lattice replace Al atoms and form replacement solutes so as to generate a significant stress field [52] in the matrix and generate frictional resistance to dislocation slippage [53]. As can be predicted, this hindering effect on dislocation should be significantly enhanced by the addition of Cu. Thus, σSS significantly increases with the increase of Cu content and is predominant in alloys with high Cu contents.
Differed from the as-quenched alloys, the peak-aged alloys show pronounced σppt. Thus, the effect of Cu addition on the mechanical properties of alloy can be expressed as [48]:
σ0.2,P = σH-P + σSS + σppt
where σ0.2,P is the yield strength of the peak-aged alloy.
Given that the decrease in the value of σSS during precipitation is quite small, σppt can be estimated by the strength difference between the as-quenched and peak-aged alloys, which can be calculated according to the following equation:
σppt ≈ σ0.2,P − σ0.2,Q
According to Equation (4), the values of σppt for Alloys 1–4 are calculated to be 96.7, 99.4, 116.1, and 122.2 MPa, respectively (Figure 22) which are greater than the corresponding values of σH-P and σSS, except for that of σSS in Alloy 4, besides, the σppt values in θ′-precipitates-contained alloys (Alloys 3 and 4) are greater than those of alloys without θ′ precipitates (Alloys 1 and 2). In particular, Alloy 4 has the largest amount of θ′ precipitation and has the largest increase in the value of σppt. This implies that the θ′ phase exerts the greatest effect on the increase in strength of the alloy. β″ precipitate is the predominant precipitate in Alloy 1, but the strength change of Alloy 1 is the smallest. Besides, with the number density of β″ precipitates decreasing and that of the Q′ precipitates increasing (Alloy 2), there is an increase in the strength of the alloy. This indicates that the Q′ precipitate has a more pronounced strengthening effect than that of the β″ precipitate.
It should be pointed out that, the value of σSS is calculated to be larger than the value of σppt in Alloy 4, which means σSS is predominant when the Cu content increases to 4.5 wt.%. This agrees with the findings of Zeren et al. [11] and Wang et al. [18] show that the strengths of as-quenched alloys (without σppt), with a relatively high Cu contents (≥4.0 wt.%) are almost equal to, or even higher than, those of peak-aged alloys with relatively low Cu contents (≤1.0 wt.%)
To sum up, the θ′ phase confers the best strengthening effect on alloys, followed by the Q′ phase and the β″ phase. As shown in Figure 19, the θ′ precipitate has a coherency interface with Al matrix, which can produce an apparent strain and significantly hinder dislocation movement. In addition, the lamellar θ′ phases are densely distributed in the alloy on {200} planes of the Al matrix (Figure 23a). It is known that the main slip system of fcc Al is {111}<110>, in section on a {111}Al slip plane and the lamellar θ′ precipitates will form a triangular array in the manner shown in Figure 23b. This could also trap the dislocation therein [54], therefore, θ′ precipitates have a remarkable strengthening effect on Al alloy. Other than θ′ precipitate, the projection shapes of β″ and Q′ precipitates in the {111}Al plane are roughly circular and hexagonal respectively, (Figure 23c–f), which have a weak effect on trapping dislocations. This might account for the remarkably smaller increase in the σppt values for Alloys 1,2 than those for Alloys 3,4.
For such small precipitates in the peak-aged alloys, the increment in the strength can be estimated using the Orowan cutting mechanism [20].
σ ppt r
where r is the radius of an average equivalent circular cross section of precipitates. Under peak-aging condition, the Q′ precipitate (Figure 15a) is obviously larger than β″ precipitate (Figure 12a) which might explain the more significant strengthening effect of Q′ precipitate.
The rates of increase in strength caused by precipitation can be described by σppt0.2,Q, as shown in Figure 22, Alloy 1 has the largest value of σppt0.2,Q (58.7%), but Alloy 4 has the smallest value of σpptQ (38.1%). This indicates that the rate of increase of strength caused by precipitation of the θ′ phase is the smallest, while that caused by precipitation of the β″phase is the largest.

4.2.2. Elongation

The elongation continues decreasing with the increase of Cu content, in both as-quenched, and peak-aged, alloys.
For as-quenched alloys, their elongation is mainly affected by grain size and coarse second-phase particles [54], which can be expressed as follows:
δQ = δGR + δCS
where δQ is the elongation of as-quenched alloy, δGR is the elongation increment contributed from grain refinement, and δCS denotes the elongation increment related to the coarse second-phase.
Generally, a Cu addition can produce grain refinement, which is beneficial to the plasticity of the alloy (namely, δGR > 0). However, the increase in the amount of coarse second-phase particles, led by a Cu addition, is known to be deleterious to the plasticity of alloys (namely, δCS < 0), due to their brittleness and incoherent interfaces with the matrix [28]. Compared to the as-quenched Alloy 1, the changes in δQ for Alloys 2,3 are −1.6%, −9.1%, and −10.9%. This means that, with the increase of Cu content, the δCS effect on δQ is enhanced. Since coarse second-phase particles cause crack initiation and promote crack growth, the significant increase in the number of coarse second-phase particles, caused by the Cu addition, can increase the probability of crack nucleation and reduce the plasticity of alloy. Thus, δQ is more dominant in those alloys with high Cu contents.
For peak-age alloy, in addition to δGR and δCS, its elongation is also affected by the precipitates, which can be expressed as follows:
δP = δGR + δCS + δppt
where δP is the elongation of peak-aged alloy, and δppt represents the elongation increment arising from precipitation.
Since δppt is independent of both δGR and δCS, it can be described by the difference between the elongation of as-quenched and peak-aged alloys, namely
δppt = δP − δQ
According to Equation (7), δppt for Alloys 1–4 are −10.4%, −10.2%, −9.0%, and −8.5%, respectively (Figure 24). It is somewhat surprising to note that the lowest value of δppt is found in Alloy 1, where β″ precipitates dominate and the maximum value of δppt is presented in the Alloy 4, where θ′ precipitates dominate.
The rate of decrease of elongation, caused by precipitation, can be described by |Δδppt|/δQ. As shown in Figure 24, the value of |Δδppt|/δQ for Alloy 4 equals to 46.0% which is the greatest among these four alloys, while, the value of |Δδppt|/δQ for Alloy 1 is to 35.0% (the smallest thereof).
In summary, among these four alloys, the precipitation of the β″-phase in peak-aged Alloy 1 causes the largest reduction in elongation, but the rate of reduction is the smallest compared with those of as-quenched alloy. The precipitation of θ′-phase in peak-aged Alloy 4 leads to the smallest reduction in elongation, while the rate of reduction is the largest compared with those of as-quenched alloy. The largest reduction caused by θ′-precipitation is probably related to its trapping effect on dislocations (Figure 23b), which weakens the density of mobile dislocations in alloys and makes it difficult to activate the slip systems.
It should be pointed out that, according to our study, the difference between β″- and Q′- precipitates, in terms of their effect on elongation, is quite small. For alloys with relatively low Cu contents, it is possible to increase the elongation by increasing the Cu content if the δGR is sufficiently large. This might account for the results of Jin et al. [5] and Zhong et al. [13] showing that even a small Cu addition increases both the strength and ductility of Al-Mg-Si-Cu alloys.

5. Conclusions

A systematic study was performed on the evolution of the microstructural features and strengthening mechanisms of Al-Mg-Si-xCu alloys with different Cu contents, and the following conclusions were drawn:
(1) The Cu content exerts a grain refinement effect on both as-extruded and as-quenched Al-Mg-Si-Cu alloys. As the Cu content increases from 0.5 to 4.5 wt.%, the grain size decreases from 765 to 190 μm in the as-extruded state and from 482 to 108 μm in as-quenched state.
(2) With the increase of Cu content, the main types of precipitates of alloys change from a β″-phase in 0.5 wt.% Cu alloy to a β″-phase and a Q′-phase in 1.0 wt.% Cu alloy, Q′-phase and θ′-phase in 2.5 wt.% Cu alloy, and θ′-phase with a small amount of Q′-phase in the 4.5 wt.% Cu alloy.
(3) Cu addition decreases the solubility of Si in the Al matrix, which suppresses the nucleation of β″precipitates and leads to the relatively low density of β″ precipitates in Alloy 2.
(4) Mg influences the interfacial structure of the θ′-phase and increases occupancy of interstitial sites at the coherent interface with the Al matrix.
(5) Cu addition plays an essential role on σH-P, σSS, and σppt of Al-Mg-Si-Cu alloys. In as-quenched state, σSS is predominant in alloys with a high Cu content (≥2.5 wt.%) but is of equivalent importance as σH-P in alloy with a low Cu content (≤1.0 wt.%). In peak-aged state, σppt is dominant in alloys with Cu content ≤2.5 wt.% but σSS is predominant in alloys with 4.5 wt.% Cu content.
(6) Among the four peak-aged alloys, the precipitation of θ′-phase in Alloy 4 leads to the largest increase amplitude while the precipitation of β″-phase in Alloy 1 causes the smallest increase amplitude in σ0.2. Compared with as-quenched alloys, the rate of increase of σ0.2 attributed to θ′-phase precipitation in Alloy 4 is the smallest, while the rate of increase of σ0.2 induced by β″-phase precipitation in Alloy 1 is the largest.

Author Contributions

Conceptualization, Y.C. and Q.H.; formal analysis, H.Z. and X.L.; investigation, S.P., H.L. and W.L.; writing—original draft, Y.C.; writing—review and editing, Q.H., B.Z. and X.L.

Funding

This research was funded by National Natural Science Foundation of China (Grant Nos. 51405153 and 51875197).

Acknowledgments

We thank D.Y. Yin and Q. Xiao for their helpful discussions in this research.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Chen, Y.Q.; Pan, S.P.; Tang, S.W.; Liu, W.H.; Tang, C.P.; Xu, F.Y. Formation mechanisms and evolution of precipitate-free zones at grain boundaries in an Al-Cu-Mg-Mn alloy during homogenization. J. Mater. Sci. 2016, 51, 7780–7792. [Google Scholar] [CrossRef]
  2. Liu, C.; Liu, Y.L.; Ma, L.Y.; Yi, J.H. Effects of solution treatment on microstructure and high-cycle fatigue properties of 7075 aluminum alloy. Metals 2017, 7, 193. [Google Scholar] [CrossRef]
  3. Chen, Y.Q.; Pan, S.P.; Zhu, B.X.; Liu, X.; Liu, W.H.; Tang, S.W. The evolution of orientation relationships during the transformation of a twin-free T-particle to tenfold T-twins in an Al alloy during homogenisation. Mater. Charact. 2018, 141, 59–73. [Google Scholar] [CrossRef]
  4. Yin, D.; Xiao, Q.; Chen, Y.; Liu, H.; Yi, D.; Wang, B.; Pan, S. Effect of natural ageing and pre-straining on the hardening behaviour and microstructural response during artificial ageing of an Al-Mg-Si-Cu alloy. Mater. Des. 2016, 95, 329–339. [Google Scholar] [CrossRef]
  5. Jin, M.; Li, J.; Shao, G.J. Study of Cu addition on precipitation behaviors and mechanical properties in AA6082 Al-Mg-Si alloy. Mater. Sci. Forum 2007, 546–549, 825–828. [Google Scholar] [CrossRef]
  6. Aversa, A.; Marchese, G.; Manfredi, D.; Lorusso, M.; Calignano, F.; Biamino, S.; Lombardi, M.; Paolo Fino, P.; Pavese, M. Laser powder bed fusion of a high strength Al-Si-Zn-Mg-Cu alloy. Metals 2018, 8, 300. [Google Scholar] [CrossRef]
  7. Ferguson, J.B.; Lopez, H.; Cho, K.; Kim, C.S. Temperature effects on the tensile properties of precipitation-hardened Al-Mg-Cu-Si alloys. Metals 2016, 6, 43. [Google Scholar] [CrossRef]
  8. Shabestari, S.G.; Moemeni, H. Effect of copper and solidification conditions on the microstructure and mechanical properties of Al-Si-Mg alloys. J. Mater. Process. Technol. 2004, 153–154, 193–198. [Google Scholar] [CrossRef]
  9. Zheng, Y.; Xiao, W.; Ge, S.; Zhao, W.; Hanada, S.; Ma, C. Effects of Cu content and Cu/Mg ratio on the microstructure and mechanical properties of Al-Si-Cu-Mg alloys. J. Alloys Compd. 2015, 649, 291–296. [Google Scholar] [CrossRef]
  10. Farkoosh, A.R.; Pekguleryuz, M. Enhanced mechanical properties of an Al–Si–Cu–Mg alloy at 300 °C: Effects of Mg and the Q-precipitate phase. Mater. Sci. Eng. A 2015, 621, 277–286. [Google Scholar] [CrossRef]
  11. Zeren, M. Effect of copper and silicon content on mechanical properties in Al–Cu–Si–Mg alloys. J. Mater. Process Technol. 2005, 169, 292–298. [Google Scholar] [CrossRef]
  12. Grosselle, F.; Timelli, G.; Bonollo, F. Doe applied to microstructural and mechanical properties of Al–Si–Cu–Mg casting alloys for automotive applications. Mater. Sci. Eng. A 2010, 527, 3536–3545. [Google Scholar] [CrossRef]
  13. Zhong, H.; Rometsh, P.; Estrin, Y. Effect of alloy composition and heat treatment on mechanical performance of 6xxx aluminum alloys. T. Nonferr. Metal. Soc. 2014, 24, 2174–2178. [Google Scholar] [CrossRef]
  14. Lu, T.; Wu, J.; Pan, Y.; Tao, S.; Chen, Y. Optimizing the tensile properties of Al–11Si–0.3Mg alloys: Role of Cu addition. J. Alloys Compd. 2015, 631, 276–282. [Google Scholar] [CrossRef]
  15. Watanabe, K.; Maruno, S.; Matsuda, K.; Lee, S.; Horita, Z.; Terada, D.; Saikawa, S.; Hirosawa, S. Aging behavior and microstructure of aged excess Mg type Al-Mg-Si alloys after HPT processing. J. Jpn. Inst. Light Met. 2013, 63, 406–412. [Google Scholar] [CrossRef]
  16. Sauvage, X.; Lee, S.; Matsuda, K.; Horita, Z. Origin of the influence of Cu or Ag micro-additions on the age hardening behavior of ultrafine-grained Al-Mg-Si alloys. J. Alloys Compd. 2017, 710, 199–204. [Google Scholar] [CrossRef]
  17. Salleh, M.S.; Omar, M.Z. Influence of Cu content on microstructure and mechanical properties of thixoformed Al-Si-Cu-Mg alloys. Trans. Nonferr. Metal. Soc. 2015, 25, 3523–3538. [Google Scholar] [CrossRef]
  18. Wang, G.; Sun, Q.; Feng, L.; Hui, L.; Jing, C. Influence of Cu content on ageing behavior of AlSiMgCu cast alloys. Mater. Des. 2007, 28, 1001–1005. [Google Scholar] [CrossRef]
  19. Hutchinson, C.R.; Ringer, S.P. Precipitation processes in Al-Cu-Mg alloys microalloyed with Si. Metall. Mater. Trans. A 2000, 31, 2721–2733. [Google Scholar] [CrossRef]
  20. Esmaeili, S.; Lloyd, D.J.; Poole, W.J. A yield strength model for the Al-Mg-Si-Cu alloy AA6111. Acta Mater. 2003, 51, 2243–2257. [Google Scholar] [CrossRef]
  21. Miao, W.F.; Laughlin, D.E. Effects of Cu content and preaging on precipitation characteristics in aluminum alloy 6022. Metall. Mater. Trans. A 2000, 31, 361–371. [Google Scholar] [CrossRef] [Green Version]
  22. Jiang, X.; Galano, M.; Audebert, F. Extrusion textures in Al, 6061 alloy and 6061/SiCp nanocomposites. Mater. Charact. 2014, 88, 111–118. [Google Scholar] [CrossRef]
  23. Gras, C.; Meredith, M.; Hunt, J.D. Microdefects formation during the twin-roll casting of Al-Mg-Mn aluminium alloys. J. Mater. Process. Technol. 2005, 167, 62–72. [Google Scholar] [CrossRef]
  24. Zhuang, L.; Bottema, J.; Kaasenbrood, P.; Miller, W.S.; Smet, P.D. The effect of small particles on annealed grain size and texture of Al-Mg-Si alloys. Mater. Sci. Forum 1996, 217–222, 487–492. [Google Scholar] [CrossRef]
  25. Farkoosh, A.R.; Javidani, M.; Hoseini, M.; Larouche, D.; Pekguleryuz, M. Phase formation in as-solidified and heat-treated Al-Si-Cu-Mg-Ni alloys: Thermodynamic assessment and experimental investigation for alloy design. J. Alloys Compd. 2013, 551, 596–606. [Google Scholar] [CrossRef]
  26. Song, Y.F.; Ding, X.F.; Xiao, L.R.; Zhao, X.J.; Cai, Z.Y.; Gguo, L.; Li, Y.W.; Zheng, Z.Z. Effects of two-stage aging on the dimensional stability of Al-Cu-Mg alloy. J. Alloys Compd. 2017, 701, 508–514. [Google Scholar] [CrossRef]
  27. Guo, M.X.; Zhu, J.; Zhang, Y.; Li, G.J.; Lin, T.; Zhang, J.S.; Zhuang, L.Z. The formation of bimodal grain size distribution in Al-Mg-Si-Cu alloy and its effect on the formability. Mater. Charact. 2017, 132, 248–259. [Google Scholar] [CrossRef]
  28. Wang, S.C.; Starink, M.J. Precipitates and intermetallic phases in precipitation hardening Al-Cu-Mg-(Li) based alloys. Int. Mater. Rev. 2005, 50, 193–215. [Google Scholar] [CrossRef]
  29. Bourgeois, L.; Dwyer, C.; Weyland, M.; Nie, J.F.; Muddle, B.C. Structure and energetics of the coherent interface between the θ′ precipitate phase and aluminium in Al-Cu. Acta Mater. 2011, 59, 7043–7050. [Google Scholar] [CrossRef]
  30. Wolverton, C.; Ozoliņš, V. Entropically favored ordering: The metallurgy of Al2Cu revisited Revisited. Phys. Rev. Lett. 2001, 86, 5518–5521. [Google Scholar] [CrossRef] [PubMed]
  31. Wolverton, C. Crystal structure and stability of complex precipitate phases in Al-Cu-Mg-(Si) and Al-Zn-Mg alloys. Acta Mater. 2001, 49, 3129–3142. [Google Scholar] [CrossRef]
  32. Bourgeois, L.; Dwyer, C.; Weyland, M.; Nie, J.F.; Muddle, B.C. The magic thicknesses of θ′ precipitates in Sn-microalloyed Al-Cu. Acta Mater. 2012, 60, 633–644. [Google Scholar] [CrossRef]
  33. Matsuda, K.; Ikeno, S.; Sato, T.; Uetani, Y. New quaternary grain boundary precipitate in Al-Mg-Si alloy containing silver. Scr. Mater. 2006, 55, 127–129. [Google Scholar] [CrossRef]
  34. Troeger, L.P.; Starke, E.A. Particle-stimulated nucleation of recrystallization for grain-size control and superplasticity in an Al-Mg-Si-Cu alloy. Mater. Sci. Eng. A 2000, 293, 19–29. [Google Scholar] [CrossRef]
  35. Mikhaylovskaya, A.V.; Ryazantseva, M.A.; Portnoy, V.K. Effect of eutectic particles on the grain size control and the superplasticity of aluminium alloys. Mater. Sci. Eng. A 2011, 528, 7306–7309. [Google Scholar] [CrossRef]
  36. Moghanaki, S.K.; Kazeminezhad, M.; Logé, R. Recrystallization behavior of multi-directionally forged over-aged and solution treated Al-Cu-Mg alloy during non-isothermal annealing. Mater. Des. 2017, 132, 250–256. [Google Scholar] [CrossRef]
  37. Chakrabarti, D.J.; Laughlin, D.E. Phase relations and precipitation in Al-Mg-Si alloys with Cu additions. Prog. Mater. Sci. 2004, 49, 389–410. [Google Scholar] [CrossRef]
  38. Tsao, C.S.; Chen, C.Y.; Jeng, U.S.; Kuo, T.Y. Precipitation kinetics and transformation of metastable phases in Al-Mg-Si alloys. Acta Mater. 2006, 54, 4621–4631. [Google Scholar] [CrossRef]
  39. Chen, J.H.; Costan, E.; Huis, M.A.V.; Xu, Q.; Zandbergen, H.W. Atomic pillar-based nanoprecipitates strengthen Al-Mg-Si alloys. Science 2006, 312, 416–419. [Google Scholar] [CrossRef] [PubMed]
  40. Edwards, G.A.; Stiller, K.; Dunlop, G.L.; Couper, M.J. The precipitation sequence in Al-Mg-Si alloys. Acta Mater. 1998, 46, 3893–3904. [Google Scholar] [CrossRef]
  41. Dumolt, S.D.; Laughlin, D.E.; Williams, J.C. Formation of a modified β″ phase in aluminium alloy 6061. Scr. Metal. 1984, 18, 1347–1350. [Google Scholar] [CrossRef]
  42. Torsæter, M.; Lefebvre, W.; Marioara, C.D.; Andersen, S.J.; Walmsley, J.C.; Holmestad, R. Study of intergrown L and Q′ precipitates in Al-Mg-Si-Cu alloys. Scr. Mater. 2011, 64, 817–820. [Google Scholar] [CrossRef]
  43. Perovic, A.; Perovic, D.D.; Weatherly, G.C.; Lloyd, D.J. Precipitation in aluminum alloys AA6111 and AA6016. Scr. Mater. 1999, 41, 703–708. [Google Scholar] [CrossRef]
  44. Saito, T.; Marioara, C.D.; Andersen, S.J.; Lefbvre, W.; Holmestad, R. Aberration-corrected HAADF-STEM investigations of precipitate structures in Al–Mg–Si alloys with low Cu additions. Philos. Mag. Ser. 2014, 94, 520–531. [Google Scholar] [CrossRef]
  45. Raviprasad, K.; Hutchinson, C.R.; Sakurai, T.; Ringer, S.P. Precipitation processes in an Al-2.5Cu-1.5Mg (wt.%) alloy microalloyed with Ag and Si. Acta Mater. 2003, 51, 5037–5050. [Google Scholar] [CrossRef]
  46. Ringer, S.P.; Hono, K.; Polmear, I.J.; Sakurai, T. Nucleation of precipitates in aged Al-Cu-Mg-(Ag) alloys with high Cu:Mg ratios. Acta Mater. 1996, 44, 1883–1898. [Google Scholar] [CrossRef]
  47. Liu, L.; Chen, J.H.; Wang, S.B.; Liu, C.H.; Yang, S.S.; Wu, C.L. The effect of Si on precipitation in Al-Cu-Mg alloy with a high Cu/Mg ratio. Mater. Sci. Eng. A 2014, 606, 187–195. [Google Scholar] [CrossRef]
  48. Huskins, E.L.; Cao, B.; Ramesh, K.T. Strengthening mechanisms in an Al-Mg alloy. Mater. Sci. Eng. A 2010, 527, 1292–1298. [Google Scholar] [CrossRef]
  49. Hansen, N. Hall-petch relation and boundary strengthening. Scripta Mater. 2004, 51, 801–806. [Google Scholar] [CrossRef]
  50. Kendig, K.L.; Miracle, D.B. Strengthening mechanisms of an Al-Mg-Sc-Zr alloy. Acta Mater. 2002, 50, 4165–4175. [Google Scholar] [CrossRef]
  51. Zhu, Z.; Han, J.; Gao, C.; Liu, M.; Song, J.; Wang, Z.; Li, H. Microstructures and mechanical properties of Al-Li 2198-T8 alloys processed by two different severe plastic deformation methods: A comparative study. Mater. Sci. Eng. A 2017, 681, 65–73. [Google Scholar] [CrossRef]
  52. Srivatsan, T.; Kolar, D.; Magnusen, P. The cyclic fatigue and final fracture behavior of aluminum alloy 2524. Mater. Des. 2002, 23, 129–139. [Google Scholar] [CrossRef]
  53. Zheng, Z.Q.; Cai, B.; Zhai, T.; Li, S.C. The behavior of fatigue crack initiation and propagation in AA2524-T34 alloy. Mater. Sci. Eng. A 2011, 528, 2017–2022. [Google Scholar] [CrossRef]
  54. Nie, J.F.; Muddle, B.C. Strengthening of an Al–Cu–Sn alloy by deformation-resistant precipitate plates. Acta Mater. 2008, 26, 3490–3501. [Google Scholar] [CrossRef]
Figure 1. Sample size for tensile testing (unit: mm).
Figure 1. Sample size for tensile testing (unit: mm).
Metals 09 00524 g001
Figure 2. Optical micrographs of alloys at different states: (a) as-extruded Alloy 1, (b) as-quenched Alloy 1, (c) as-extruded alloy 2, (d) as-quenched Alloy 2, (e) as-extruded Alloy 3, (f) as-quenched Alloy 3, (g) as-extruded alloy 4, (h) as-quenched Alloy 4.
Figure 2. Optical micrographs of alloys at different states: (a) as-extruded Alloy 1, (b) as-quenched Alloy 1, (c) as-extruded alloy 2, (d) as-quenched Alloy 2, (e) as-extruded Alloy 3, (f) as-quenched Alloy 3, (g) as-extruded alloy 4, (h) as-quenched Alloy 4.
Metals 09 00524 g002
Figure 3. The {200} pole figures of four as-quenched alloys: (a) Alloy 1 (b) Alloy 2 (c) Alloy 3 (d) Alloy 4.
Figure 3. The {200} pole figures of four as-quenched alloys: (a) Alloy 1 (b) Alloy 2 (c) Alloy 3 (d) Alloy 4.
Metals 09 00524 g003
Figure 4. Back-scattered electron (BSE) images of the alloys at different states: (a) as-extruded Alloy 1, (b) as-quenched Alloy 1, (c) as-extruded Alloy 2, (d) as-quenched Alloy 2, (e) as-extruded Alloy 3, (f) as-quenched Alloy 3, (g) as-extruded Alloy 4, (h) as-quenched Alloy 4.
Figure 4. Back-scattered electron (BSE) images of the alloys at different states: (a) as-extruded Alloy 1, (b) as-quenched Alloy 1, (c) as-extruded Alloy 2, (d) as-quenched Alloy 2, (e) as-extruded Alloy 3, (f) as-quenched Alloy 3, (g) as-extruded Alloy 4, (h) as-quenched Alloy 4.
Metals 09 00524 g004
Figure 5. Elemental mapping of the as-extruded Alloy 1 examined by EPMA.
Figure 5. Elemental mapping of the as-extruded Alloy 1 examined by EPMA.
Metals 09 00524 g005
Figure 6. Elemental mapping of the as-quenched Alloy 1 examined by EPMA.
Figure 6. Elemental mapping of the as-quenched Alloy 1 examined by EPMA.
Metals 09 00524 g006
Figure 7. Elemental mapping of the as-extruded Alloy 4 examined by EPMA.
Figure 7. Elemental mapping of the as-extruded Alloy 4 examined by EPMA.
Metals 09 00524 g007
Figure 8. Elemental mapping of the as-quenched Alloy 4 examined by EPMA.
Figure 8. Elemental mapping of the as-quenched Alloy 4 examined by EPMA.
Metals 09 00524 g008
Figure 9. Hardness versus aging time at 165 °C of Al-Mg-Si alloys with different Cu contents.
Figure 9. Hardness versus aging time at 165 °C of Al-Mg-Si alloys with different Cu contents.
Metals 09 00524 g009
Figure 10. Tensile curves of the alloys in different heat-treatment states: (a) as-quenched, (b) peak-aged.
Figure 10. Tensile curves of the alloys in different heat-treatment states: (a) as-quenched, (b) peak-aged.
Metals 09 00524 g010
Figure 11. TEM and SADP images of the four peak-aged Al-Mg-Si-Cu alloys observed in the <010>Al projection: (a,b,c) Alloy 1, (d,e,f) Alloy 2, (g,h,i) Alloy 3, (j,k,l) Alloy 4.
Figure 11. TEM and SADP images of the four peak-aged Al-Mg-Si-Cu alloys observed in the <010>Al projection: (a,b,c) Alloy 1, (d,e,f) Alloy 2, (g,h,i) Alloy 3, (j,k,l) Alloy 4.
Metals 09 00524 g011
Figure 12. Granular-shaped precipitate in the peak-aged Alloy 1 (165 °C/360 min) observed via the <010>Al direction: (a) HRTEM image; (b) corresponding fast Fourier transform (FFT); (c) simulated pattern.
Figure 12. Granular-shaped precipitate in the peak-aged Alloy 1 (165 °C/360 min) observed via the <010>Al direction: (a) HRTEM image; (b) corresponding fast Fourier transform (FFT); (c) simulated pattern.
Metals 09 00524 g012
Figure 13. Acicular precipitate in the peak-aged Alloy 1 (165 °C/360 min) observed via the <010>Al direction: (a) HRTEM image; (b) corresponding FFT; (c) simulated pattern.
Figure 13. Acicular precipitate in the peak-aged Alloy 1 (165 °C/360 min) observed via the <010>Al direction: (a) HRTEM image; (b) corresponding FFT; (c) simulated pattern.
Metals 09 00524 g013
Figure 14. Acicular precipitate in the peak-aged Alloy 2 (165 °C/480 min) observed via the <010>Al direction: (a) HRTEM image; (b) corresponding FFT; (c) simulated pattern.
Figure 14. Acicular precipitate in the peak-aged Alloy 2 (165 °C/480 min) observed via the <010>Al direction: (a) HRTEM image; (b) corresponding FFT; (c) simulated pattern.
Metals 09 00524 g014
Figure 15. Granular-shaped, Q′-phase precipitate in the peak-aged Alloy 2 (165 °C/480 min) observed via the <010>Al direction: (a) HRTEM image; (b) corresponding FFT; (c) simulated pattern.
Figure 15. Granular-shaped, Q′-phase precipitate in the peak-aged Alloy 2 (165 °C/480 min) observed via the <010>Al direction: (a) HRTEM image; (b) corresponding FFT; (c) simulated pattern.
Metals 09 00524 g015
Figure 16. HAADF-STEM images and corresponding EDS mapping of peak-aged Alloy 3 (165 °C/540 min) observed via the <010>Al direction.
Figure 16. HAADF-STEM images and corresponding EDS mapping of peak-aged Alloy 3 (165 °C/540 min) observed via the <010>Al direction.
Metals 09 00524 g016
Figure 17. HRTEM image and corresponding FFT of lamellar precipitates in the peak-aged Alloy 3 (165 °C/540 min) observed via the <010>Al direction.
Figure 17. HRTEM image and corresponding FFT of lamellar precipitates in the peak-aged Alloy 3 (165 °C/540 min) observed via the <010>Al direction.
Metals 09 00524 g017
Figure 18. High-resolution HAADF-STEM images of Alloy 4 (165 °C/960 min) observed via the <010>Al zone axis. (a) The lamellar θ′ precipitates; (b) Z-contrast image of the θ′ phase; (c) the granulated Q′ precipitate; (d) Z-contrast image of the Q′ phase.
Figure 18. High-resolution HAADF-STEM images of Alloy 4 (165 °C/960 min) observed via the <010>Al zone axis. (a) The lamellar θ′ precipitates; (b) Z-contrast image of the θ′ phase; (c) the granulated Q′ precipitate; (d) Z-contrast image of the Q′ phase.
Metals 09 00524 g018
Figure 19. The interface of the θ´ phase in Figure 18b. (a) Z-contrast image; (b) image intensity profiles; (c) schematic diagram of the atomic positions.
Figure 19. The interface of the θ´ phase in Figure 18b. (a) Z-contrast image; (b) image intensity profiles; (c) schematic diagram of the atomic positions.
Metals 09 00524 g019
Figure 20. Granular-shaped Q′ precipitate in peak-aged Alloy 4 (165°C/960 min) observed via the <010>Al direction: (a) HRTEM image, (b) corresponding FFT, and (c) simulated pattern.
Figure 20. Granular-shaped Q′ precipitate in peak-aged Alloy 4 (165°C/960 min) observed via the <010>Al direction: (a) HRTEM image, (b) corresponding FFT, and (c) simulated pattern.
Metals 09 00524 g020
Figure 21. Schematic drawings illustrating the microstructure of the peak-aged four alloys (a) Alloy 1, (b) Alloy 2; (c) Alloy 3, and (d) Alloy 4.
Figure 21. Schematic drawings illustrating the microstructure of the peak-aged four alloys (a) Alloy 1, (b) Alloy 2; (c) Alloy 3, and (d) Alloy 4.
Metals 09 00524 g021
Figure 22. Influence of precipitation on the strength of the alloy.
Figure 22. Influence of precipitation on the strength of the alloy.
Metals 09 00524 g022
Figure 23. Schematic diagrams showing (a) distribution of lamellar β″ precipitates in the Al matrix and (b) projection of the intersected β″ precipitates in a {111}Al plane (c) distribution of lamellar Q′ precipitates in the Al matrix and (d) projection of the intersected Q′ precipitates in a {111}Al plane (e) distribution of lamellar θ′ precipitates in the Al matrix and (f) projection of the intersected θ′ precipitates in a {111}Al plane.
Figure 23. Schematic diagrams showing (a) distribution of lamellar β″ precipitates in the Al matrix and (b) projection of the intersected β″ precipitates in a {111}Al plane (c) distribution of lamellar Q′ precipitates in the Al matrix and (d) projection of the intersected Q′ precipitates in a {111}Al plane (e) distribution of lamellar θ′ precipitates in the Al matrix and (f) projection of the intersected θ′ precipitates in a {111}Al plane.
Metals 09 00524 g023
Figure 24. Influence of precipitation on the elongation of the alloy.
Figure 24. Influence of precipitation on the elongation of the alloy.
Metals 09 00524 g024
Table 1. Chemical compositions of the alloys (wt.%).
Table 1. Chemical compositions of the alloys (wt.%).
No.MgSiCuMnCrZnTiFeAl
10.420.500.500.200.100.200.02<0.10Bal.
20.420.501.000.200.100.200.02<0.10Bal.
30.420.502.500.200.100.200.02<0.10Bal.
40.420.504.500.200.100.200.02<0.10Bal.
Table 2. Average grain size (AGZs) and grain aspect ratio (GARs) of four Al-Mg-Si-Cu alloys at different states.
Table 2. Average grain size (AGZs) and grain aspect ratio (GARs) of four Al-Mg-Si-Cu alloys at different states.
Sample StateAs-Extruded StateAs-Quenched
Sample No.Alloy 1Alloy 2Alloy 3Alloy 4Alloy 1Alloy 2Alloy 3Alloy 4
AGZ (µm)765538475190482351211108
GAR6.478.279.6711.232.352.973.564.12

Share and Cite

MDPI and ACS Style

Chen, Y.; Hu, Q.; Pan, S.; Zhang, H.; Liu, H.; Zhu, B.; Liu, X.; Liu, W. Influences of Cu Content on the Microstructure and Strengthening Mechanisms of Al-Mg-Si-xCu Alloys. Metals 2019, 9, 524. https://doi.org/10.3390/met9050524

AMA Style

Chen Y, Hu Q, Pan S, Zhang H, Liu H, Zhu B, Liu X, Liu W. Influences of Cu Content on the Microstructure and Strengthening Mechanisms of Al-Mg-Si-xCu Alloys. Metals. 2019; 9(5):524. https://doi.org/10.3390/met9050524

Chicago/Turabian Style

Chen, Yuqiang, Qiang Hu, Suping Pan, Hao Zhang, Huiqun Liu, Biwu Zhu, Xiao Liu, and Wenhui Liu. 2019. "Influences of Cu Content on the Microstructure and Strengthening Mechanisms of Al-Mg-Si-xCu Alloys" Metals 9, no. 5: 524. https://doi.org/10.3390/met9050524

APA Style

Chen, Y., Hu, Q., Pan, S., Zhang, H., Liu, H., Zhu, B., Liu, X., & Liu, W. (2019). Influences of Cu Content on the Microstructure and Strengthening Mechanisms of Al-Mg-Si-xCu Alloys. Metals, 9(5), 524. https://doi.org/10.3390/met9050524

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop