The Role of Nano-TiO2 Lubricating Fluid on the Hot Rolled Surface and Metallographic Structure of SS41 Steel

1
School of Materials Science and Engineering, University of Science and Technology Beijing, Beijing 100083, China
2
Departments of Foundational Science, Beijing Union University, Beijing 100101, China
*
Author to whom correspondence should be addressed.
Nanomaterials 2018, 8(2), 111; https://doi.org/10.3390/nano8020111
Submission received: 22 January 2018 / Accepted: 11 February 2018 / Published: 16 February 2018

Abstract

:
In this paper, nano-TiO2lubricating fluid was chosen as an advanced rolling lubricant to investigate its effect on the hot rolled surface and metallographic structure of SS41 steel strips. The tribological performances of nano-TiO2 lubricating fluid were measured by a four-ball tribotester. The hot rolling experiments under different lubrication conditions were carried out by a four-high rolling mill. The surface morphology, oxide scales and metallographic structure after hot rolling were observed using a confocal laser scanning microscope and scanning electron microscope (SEM), respectively. The composition of surface attachments was analyzed with X-ray photoelectron spectroscopy (XPS). The results indicate that the nano-TiO2 lubricating fluid has a better tribological performance. The surface defects on the hot rolled surface could be decreased. The phase composition of the surface still appears as a mixture of ferrite and pearlite. The surface of steel strips is not micro-alloyed with titanium as predicted. Additionally, the grain size of rolled steel strips which were lubricated with the nano-TiO2lubricating fluid decreased by nearly 50%, compared with traditional lubricating fluid. Furthermore, it was found that the thickness of the oxide layers on the surface reduced, whilst the Rockwell hardness of the oxide layers was enhanced as nano-TiO2 lubricating fluid was applied.

1. Introduction

Due to their special physical and chemical properties [1], such as excellent diffusivity, chemical activity, and the ability to self-repair and film-form [2], nanoparticles have extensive applications in lubrication. Nanoparticles, such as molybdenum disulfide (MoS2) [3,4], silicon dioxide (SiO2) [3,5], titanium dioxide (TiO2) [6,7,8] and aluminum oxide (Al2O3) [8], can create the appropriate conditions for machining process [9]. Recent studies have confirmed that nanoparticles have potential applications in the steel rolling process [10,11], machine cutting process [12,13,14], micro-drilling process [15], etc. Previous studies reported that nano-TiO2 has good friction-reducing, anti-wear, and cooling properties, so it can reduce the coefficient of friction and rolling force during the hot rolling process [16,17].
Although previous studies have verified that using nano-TiO2 as an additive can improve the tribological properties of lubricants, few researchers have considered the impact of heating effect during the hot rolling process. Existing studies have principally focused on the effectiveness of nano-TiO2 on the rolling force, friction coefficient and other macro-performances. In this paper, the role of nano-TiO2 lubricating fluid on the microstructure of hot-rolled metal surface was investigated with interest. As the size decreases, anatase titanium dioxide can attain a more stable shape than rutile titanium dioxide at room temperature [18] and hence, TiO2 nanoparticles used in nano-lubricating fluid are always in the anatase phase. The anatase phase is known to be metastable, while rutile is the stable phase. Therefore, the anatase phase will transform to the rutile phase under heat treatment at temperatures typically ranging between 600–900°C [19,20]. The fundamental structures of anatase phase and rutile phase nano-TiO2 are both octahedron structures consisting of titanium and oxygen elements. However, the fundamental structures of anatase nano-TiO2 are connected with the communal vertexes, while the fundamental structures of the rutile phase share the edges. Actually, there are some previous chemical bonds broken and some emerging chemical bonds formed during the heat treatment [21]. Therefore, the TiO2 nanoparticles used in nano-TiO2 lubricating fluid might have a chance to react with the surface steel during the hot rolling process and cause an inhomogeneity of the strips in structure and texture. The structural and textural inhomogeneity of steel strips would impact the processing properties and service performance of products [22].
In this paper, nano-TiO2 lubricating fluid was prepared, and its lubrication performance was evaluated, using a four-ball tribotester. The surface morphology, oxidation, metallographic structures and elemental compositions on the surface of the SS41 steel strips, lubricated with or without nano-TiO2 lubricating fluid, were compared, to explore these problems. This exploration will play an important role in the application prospect of nano-TiO2 lubricating fluid used in hot rolling.

2. Experimental

2.1. Materials

Anatase nano-TiO2 (TiO2 content, >95 wt %) with a nominal diameter of 90 nm was used as the lubricant additive in this study. To prepare uniform and stable nano-fluid, the nano-TiO2 cannot be solely added into deionized water because of the polymerization of nanoparticles [23]. Both the physical dispersion method and the chemical dispersion method were used to solve this problem. A magnetic stirrer and ultrasonic dispersion instrument were used for physical dispersion. Some water-soluble dispersants, such as sodium hexametaphosphate (SHMP) and sodium dodecyl benzene sulfonate (SDBS) have both hydrophilic groups and lipophilic groups. So, they were added for chemical dispersion. The nano-TiO2 lubricating fluid was prepared according to the formula shown in Table 1. This kind of liquid can stay stable for more than 7 days. Furthermore, traditional lubricating fluid containing every additive in Table 1, except anatase nano-TiO2, was obtained as a control group. In this work, the traditional lubricating fluid was used to determine the interference of the other additives on the results.
As the four-high rolling mill used in hot rolling test was an experimental mill with a working roller dimension of Ф170 × 350 mm, 70 mm was chosen as the breadth of the initial materials to reduce the rolling force. In addition, the steel strips (initial dimensions, 200 × 70 × 30 mm3) used in the hot rolling test were provided by Jiuquan Iron & Steel (Group) Co., Ltd. The chemical compositions of the steel strips are listed in Table 2.

2.2. Tribological Test

The tribological tests were taken to represent the tribological properties of nano-TiO2 lubricating fluid. In addition, the same tests were conducted on the traditional lubricating fluid as a control trial. The maximum non-seizure load (PB), friction coefficient and wear scar diameter were measured on an MR-S10A four-ball tribometer, equipped with a rolling friction pair. The schematic of the four-ball rolling friction is shown in Figure 1.
A rotation velocity of 1760 r/min of the upper steel ball was applied in the representation of PB. While in the wear tests, the rotation velocity of the upper steel ball was 1200 r/min, the constant load was 392 N and the testing time was 30 min. The friction coefficients during the wear tests and the wear scar diameters after the wear test were measured to verify the friction reduction and antiwear behavior of nano-TiO2 lubricating fluid.

2.3. Hot Rolling Test

The austenite phase has lower strength and hardness than the ferrite phase [24]—that is to say, the austenite phase possesses a preferable plasticity. To enhance the rolling efficiency, the hot rolling process should be taken completely in the austenitic phase. SS41 steel is a typical hypoeutectoid steel, wherefore the metallographic structure of SS41 steel is composed of a single austenite phase when the steels are heated above 800 °C. The strips were heated to 1150 °C, which is an empirical value, and held for 2 h to guarantee the temperature of the steel strips was above 850 °C during hot rolling. The nominal rolling speed was about 2.0 m/s, and the rolling pass was 5. The steel strips were hot rolled to 4 mm thick from 30 mm on the 4-high mill, and the corresponding rolling reductions were 26.7%, 27.3%, 37.5%, 40.0% and 33.3%, respectively. The sketch of hot rolling is shown in Figure 2a. Three kinds of lubricant conditions, namely, non-lubricant, traditional lubricating fluid, and nano-TiO2 lubricating fluid were used on the upper working roller in three-group comparative experiments, as shown in Figure 2b.

2.4. Characterization Methods

Four hot-rolled steel samples for each experimental group were prepared for analysis of surface morphology, oxidation, metallographic structure and surface chemical composition. The hot-rolled steel strips were cut into blocks of 10 × 10 mm from the center of the strips along the planes of the rolling direction (RD) and the normal direction (ND). The distance between each block was 20 mm.
The rolled surface of the first samples can be directly used for surface morphology and roughness observations after rinsing with petroleum ether. To provide an intuitive description of the surface quality of the hot-rolled steel strips, the surface morphology after hot rolling was characterized by a confocal laser scanning microscope (Olympus LEXTOLS 4000, Olympus, Japan) for 2D and 3D topography observation. The linear roughness perpendicular to the rolling direction was measured. To ensure the accuracy of the data, each group of the samples was measured five times and the determined value was obtained by averaging five measurements. To distinguish the form of wear, SEM (ZEISS EVO 18, Germany) was used for finer observation, and energy dispersive spectrometry (EDS, ZEISS, Germany) with a scanning electron microscope was applied to research the primary elementary composition of different forms of wear on the hot rolled surface.
The second samples used for oxidation investigation had to be milled and polished to Ra < 0.1 μm. To explore thickness of the oxide layers, the cross-sectional blocks were ground with SiC paper of 240, 400, 800, 1500 and 2000 mesh, orderly, and then polished by nylon fabric with a 2.5 mm diamond polishing paste. The oxide layers were observed by SEM with backscattered electron microscopy (BSE) and the thickness of the oxide layers were measured by EDS with elemental linear scanning. In this work, the elemental linear scanning was taken on the cross-section, with the scanning direction perpendicular to the rolled surface. The higher oxygen content represented the behavior of the oxide layers, while the lower oxygen content represented the simple metal. The Rockwell hardness of the oxide scales was conducted on a hardness tester; the applied load and holding time were 100 kg and 60 s, respectively.
The third samples were employed for the characterization of metallographic structure. The rolled surface of the samples had to be milled with SiC paper of 150 mesh to dislodge the oxide layers, and then milled and polished to Ra < 0.1 μm, using the same method mentioned in the last paragraph. After polishing, the surface was etched for 3–5 s with nitric acid alcohol, which was a mixture of 96% alcohol and 4% nitric acid, before microstructural analysis. The etched surface was surveyed by SEM, and the software of image analysis (Image Tool) was used to measure the grain size. To obtain a veracious datum, 12 adjoining grains in the image were chosen to be measured, and the average size was calculated, according to the 12 measurements. Then, the thicknesses of the samples were measured by micrometer and each final result was obtained by averaging six measurements.
The last samples were cut into thin plates, each with a thickness of 1.5 mm, for the X-ray photoelectron spectroscopy (XPS, Kratos, Japan), to determine the chemical states of typical elements on the strips’ surfaces.

3. Results and Discussion

3.1. Tribology Performance

The results of the tribology tests are shown in Table 3. The maximum non-seizure loads were measured according to GB/T 12583-1998. It can be seen in Table 3 that the maximum non-seizure load (PB) was signally enhanced by using TiO2 nanoparticles because of their remarkable film-forming property. This means the nano-TiO2 lubricating fluid can take effect under a greater positive pressure. The wear tests of each lubricant developed for 30 min, and the friction coefficients were measured and collected per second. The average friction coefficients of two lubricants were calculated to evaluate the friction reducing effect of using nano-TiO2. Wear scar diameters of the lower three steel balls were measured by optical microscope, and the mean values were calculated to evaluate the antiwear behavior of the nano-TiO2 lubricating fluid.
The friction coefficient-time curves of the traditional lubricating fluid and nano-TiO2 fluid of the upper steel ball under 392 N at 1200 r/min are shown in Figure 3. The friction coefficient of the traditional lubricating fluid presented a remarkably increasing trend with a prolonged time before 900 s and then became stable at about 0.17. As for the nano-TiO2 lubricating fluid, the friction coefficient was relatively consistent with the friction time. The results can exactly confirm the excellent film-forming property of nano-TiO2. Nano-TiO2 can easily adsorb to the steel surface to form a lubricating film. Thus, the friction coefficient-time curve of the nano-TiO2 lubricating fluid should be more stable.

3.2. Surface Morphology

The optical micrograph and three-dimensional (3D) topography of hot-rolled strips under three different lubrication states were shown in Figure 4a–c . In Figure 4, a comprehensive representation was obtained from the optical micrograph. A surface micrograph of the hot-rolled strip shows signs of larger dark regions and dense scratches as no lubricant was used. There are also many wide and deep furrows that are perpendicular to the rolling direction on the non-lubricated surface. As a traditional lubricating fluid was used, there are very few transversal furrows that can be seen in the micrograph; furthermore, the size of dark regions and the deepness of dense scratches are both abated. However, many areas that are neither dark, nor bright, are exposed on the surface lubricated with traditional lubricating fluid. These areas might be due to the oxide wear that will be discussed in the following part. All these surface defects of the hot-rolled surface could be significantly reduced when the nano-TiO2 fluid was employed. It is known that optical microscopy has an inherently small depth field, whence the dark and bright regions can be associated with height difference. It indicates that the surface roughness of the hot-rolled strips would be decreased by using nano-TiO2lubricating fluid. These conclusions are confirmed by homologous 3D topographies in Figure 4. The data in the top left corner of the 3D topographies are the linear roughnesses of samples, which correspond to the change in rule of the surface topographies.
The SEM was used to distinguish and analyze these surface defects. The SEM images are shown in Figure 5. The irregular pieces of dark regions are metals desquamated from the strip surface because of the adhesive wear between the friction pairs. These metal fragments may come off the surface on which they are formed and be transferred back to the original surface [25]. As a result, the area whose surface steel avulsed from the strips is lower (appears blue in the 3D topographies), while the area that adhered to the metal fragments is higher (appears yellow in the 3D topographies). The adhesive wear of the strip surface will markedly influence the surface quality and strip yield. The pits pinpointed in Figure 5 can coincidentally correspond to this adhesive wear. The adhesive wear was verified to be reduced by using nano-TiO2 fluid, according to these results. Due to the adhesive wear, there must be some oxide scales and other hard materials adhered to the rolls. Therefore, the appearance of dense scratches parallel to the rolling direction is on account of scratching of the oxide scales and other hard materials adhered to the rolls. Comparing the size and depth of pits on three different surfaces, it is obvious that the pits on the non-lubricated surface are the largest, the pits in the traditional fluid lubricated surface take second place, and the pits in the nano-TiO2 fluid lubricated surface are smallest and shallowest. As a consequence, the scratches in Figure 5a are wider and deeper, while the scratches in Figure 5b,c are almost invisible. Moreover, the furrows perpendicular to the rolling direction must be cracks formed by the rupture of the steel surface. A crack might be a fearful surface defect which has a serious influence on the usability of the steel strips.
As shown in Figure 4b and Figure 5b, there are many regions with distinct colors on the surface lubricated with traditional lubricating fluid. These regions are speculated to be due to oxide wear as the traditional lubricating fluid was composed mainly of water. This inference was confirmed by EDS spectra of the strip surface lubricated with the traditional lubricating fluid, in Figure 6. The oxygen content of the abnormal region is higher than the normal region. This result indicates that there were some newly generated iron oxides in the abnormal region, which verified the previous assumption.

3.3. Oxide Scales

Figure 7 illustrates oxide scales of hot-rolled strips under different lubricating conditions. The oxide scales of steel strips rolling without any lubricant are extremely loosened, as shown in the SEM image. As for the steel strips lubricated with the traditional lubricating fluid, this can hardly be improved. When nano-TiO2 fluid was used, the oxide scales become compact and fewer voids can be seen in the SEM image. The Rockwell hardness’ of the oxide scales listed in the top right corner of the SEM images are consistent with the visual results—the more compact the oxide scales are, higher the hardness is. The EDS with elemental linear scanning was taken to measure the thickness of the oxide scales, and the scanning direction is annotated on the SEM images. The vertical distributions of element Fe and element O in the transverse section were quantitated, and the spots whose oxygen content was above zero were considered to be the oxide scales. The thickness of the oxide layers without any lubrication was about 40 μm (Figure 7a). The thickness was increased to 60 μm when the traditional lubricating fluid was used (Figure 7b). In Figure 7c, the thickness decreased to 20 μm. The inferior antirust property of the traditional lubricating fluid was improved by using nano-TiO2.
In order to explain the aforementioned phenomenon, XPS spectra were recorded to investigate the chemical states of the oxide scales. As shown in Figure 8, the Fe 2p peaks appeared at 710.80 eV and 724.22 eV. According to the NIST Standard Reference Data base 20 (version 4.1), the former, combined with the O 1s peaks at 529.72 eV, is assigned to Fe3O4, while the latter, combined with the O 1 s peak at 532.05 eV, is assigned to Fe2O3. The spectrum of Ti 2p shows a peak at the binding energy of 458.69 eV, combined with the binding energy of O1s 531.16 eV, which can be attributed to the chemical state of TiO2. The TiO2 signal indicates that nano-TiO2 has been deposited on the contact surfaces and forms a physical protecting film on the flat. In other words, the TiO2 nanoparticles might adsorb on the steel surface during the hot-rolling process, meanwhile, filling in the voids of the loosen oxide scales and isolating the air to prevent further rusting of the metallic matrix. Moreover, there is not any new phase formed on the steel surface—the nano-TiO2 could only create a physical adhesion film on the oxide scales to protect the steel.

3.4. Metallographic Structure

As oxide scales of the third samples were dislodged, the metallographic structure of the metal base could be explored by SEM. The microstructures of the hot-rolled metal base after polishing and etching are shown in Figure 9. The metallographic structure of the metal base appears as a mixture of ferrite and pearlite, while the matrix phase is ferrite and the second phase in grain boundaries is pearlite. There was no novel phase formed when the nano-TiO2 was added. That means there could not have been any steel strip micro-alloyed with titanium. The reason for this inference will be explained in the following part. Furthermore, comparing Figure 9a–c , the grains are observed to be refined, obviously. The refined grains will lead to better mechanical properties and processing ability, with all else held equal [26].As the grains are subtler, the deformation can be easily coordinated—both the plasticity and tenacity can be improved. Additively, the flow stress of the steels would be enhanced; as a result, the materials could have a higher strength.
To make a quantitative comparison, the average sizes in the images were measured using the image analysis software (Image Tool); the results are shown in Table 4. The grain size of the rolled steel strips with the nano-TiO2 lubricant decreased by nearly 60% when compared with non-lubrication. In addition, the traditional lubricating fluid contributes about 25%.
The main reason for this phenomenon is the increase in rolling deformation. The finishing thicknesses and spring-back values of hot rolled steel strips were shown in Table 5. The rolling mill is known to have rebound resilience, so the actual thickness would thicker than the height of the roll gap, and the real thickness is the sum of the height of the roll gap and the spring-back value. The spring-back can be reduced by about 86.7% as the TiO2 nanoparticles are added into the lubricant, and the overall reduction in the same rolling period can be enhanced visibly. On account of the rise of rolling deformation, more and more dislocations and lattice defects appeared. As a result, the nucleation rate increased due to the enhancement of lattice distortion energy, and the grains became refined [27].
To explore the reason why no new phase appeared as the nano-TiO2 was added, the crystal structure of nano-TiO2 and oxide scales were analyzed. The element Fe on the surfaces exists in the forms, Fe3+ and Fe2+, and the titanium in nano-TiO2 is Ti4+. According to the crystal structures of TiO2, Fe2O3 and FeO (Figure 10), the ligancies of Ti4+, Fe3+ and Fe2+ are all six. This indicates that the replacement of these ions may occur, on account of the lattice imperfection. The incorporation of Ti4+ into the Fe2O3 crystal lattice during hot rolling may take place as the Ti4+ radius (0.64 Å) is close to that of Fe3+ (0.68 Å) [28]. On the other hand, the ionic radius of Fe2+ (0.78 Å) and Ti4+ (0.64 Å) have great differentials, so it is not easy for Ti4+ to pass into the crystal lattice of Fe3O4.
There are three kinds of iron oxides covered on the surface of steel strips. The outermost layer is Fe2O3 which has a loose structure; the innermost layer is FeO which is denser, and the interlayer is Fe3O4 which is a mixture of Fe2O3 and FeO. Though there might be some dissociative Ti4+ which can pass into the surface, this would exist in Fe2O3, which is a porous oxide scale covered on the steel surface. The TiO2 nanoparticles would adsorb on the hole of the oxide scale; as a consequence, there is only a chemical adhesion film created on the oxide scales, but no new phase appeared in the metal base.

4. Conclusions

The present work analyzed the surface morphology and metallographic structure of hot rolled SS41 steel, lubricated with nano-TiO2 lubricating fluid. The following conclusions were drawn from this study:
(1)
Adding nano-TiO2 in lubricating fluid was associated with a 62.5% increase in the maximum non-seizure load, a 33.8% reduction in the friction coefficient and a 47.4% reduction in the wear extent, compared with traditional lubricating fluid. Moreover, the friction coefficient-time curve of nano-TiO2 lubricating fluid became smooth in only 50 s, while that of traditional lubricating fluid presented a remarkably increasing trend till 900 s.
(2)
The grain size of rolled steel strips lubricated with nano-TiO2 lubricating fluid decreased from 18.51 μm to 7.46 μm. Additionally, the phase composition of the surface still appeared as a mixture of ferrite and pearlite. There was no iron micro-alloyed phenomenon with titanium. The homogeneity of the metal base was not destroyed.
(3)
TiO2 nanoparticles could deposit on worn surfaces in the hot rolling process. With the generation of iron oxides, nano-TiO2 was distributed in the oxide scales diffusely. The compactness of the oxide scales could be drastically enhanced, which caused a slightly increase in Rockwell hardness and a decrease in the thickness of the oxide scales, from 60 μm to 20 μm. There were fewer surface defects on the hot rolled surface.

Acknowledgments

The present study is financially supported by Beijing Natural Science Foundation (No. 2182041).

Author Contributions

Y.M. and J.S. conceived and designed the experiments; Y.M., X.Y., C.D., and P.W. performed the experiments; Y.M. and J.S. analyzed the data; P.W. provided the theoretical support; Y.M. wrote the manuscript; J.S. and C.D. revised the manuscript; all authors read and approved the final version of the manuscript.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Wu, H.; Zhao, J.W.; Xia, W.Z.; Cheng, X.W.; He, A.S.; Jung, H.Y.; Wang, L.Z.; Huang, H.; Jiao, S.H.; Huang, L.; et al. A study of the tribological behaviour of TiO2 nano-additive water-based lubricants. Tribol. Int. 2017, 109, 398–408. [Google Scholar] [CrossRef]
  2. Hsu, S.M. Nano-lubrication: Concept and design. Tribol. Int. 2004, 37, 537–545. [Google Scholar] [CrossRef]
  3. Xie, H.M.; Jiang, B.; Hu, X.Y.; Peng, C.; Guo, H.L.; Pan, F.S. Synergistic effect of MoS2 and SiO2 nanoparticles as lubricant additives for magnesium alloy–steel contacts. Nanomaterials 2017, 7, 154. [Google Scholar] [CrossRef] [PubMed]
  4. Liu, Y.R.; Hu, K.H.; Hu, E.Z.; Guo, J.H.; Han, C.L.; Hu, X.G. Double hollow MoS2 nano-spheres: Synthesis, tribological properties, and functional conversion from lubrication to photocatalysis. Appl. Surf. Sci. 2017, 392, 1144–1152. [Google Scholar]
  5. Sayuti, M.; Sarhan, A.D.D.; Salem, F. Novel uses of SiO2 nano-lubrication system in hard turning process of hardened steel AISI4140 for less tool wear, surface roughness and oil consumption. J. Clean. Prod. 2014, 67, 265–276. [Google Scholar] [CrossRef]
  6. Hu, K.H.; Xu, Y.; Hu, E.Z.; Guo, J.H.; Hu, X.G. Rolling friction performance and functional conversion from lubrication to photocatalysis of hollow spherical nano-MoS2/nano-TiO2. Tribol. Int. 2016, 104, 131–139. [Google Scholar] [CrossRef]
  7. Xia, W.Z.; Zhao, J.W.; Wu, H.; Jiao, S.H.; Jiang, Z.Y. Effects of oil-in-water based nanolubricant containing TiO2 nanoparticles on the tribological behaviour of oxidized high-speed steel. Tribol. Int. 2017, 1, 77–85. [Google Scholar] [CrossRef]
  8. Luo, T.; Wei, X.W.; Zhao, H.Y.; Cai, G.Y.; Zheng, X.Y. Tribology properties of Al2O3/TiO2 nanocomposites as lubricant additives. Ceram. Int. 2014, 40, 10103–10109. [Google Scholar] [CrossRef]
  9. Totka, B.; Lucie, S.; Petra, R.; Karolína, B.; Lukas, V.; Petr, L. The application potential of SiO2, TiO2 or Ag nanoparticles as fillers in machining process fluids. J. Clean. Prod. 2017, 142, 2237–2243. [Google Scholar]
  10. Sun, J.L.; Zhu, Z.X.; Xu, P.F. Study on the lubricating performance of nano-TiO2 in water-based cold rolling fluid. Mater. Sci. Forum 2015, 817, 219–224. [Google Scholar] [CrossRef]
  11. Zhu, Z.X.; Sun, J.L.; Niu, T.L.; Liu, N.N. Experimental research on tribological performance of water-based rolling liquid containing nano-TiO2. Proc. Inst. Mech. Eng. Part N J. Nanoeng. Nanosyst. 2015, 229, 104–109. [Google Scholar] [CrossRef]
  12. Kumar, A.S.; Kumar, A.T.; Kumar, R.S.; Rai, A.D. Tribological investigation of TiO2 nanoparticle based cutting fluid in machining under minimum quantity lubrication (MQL). Mater. Today Proc. 2015, 3, 2155–2162. [Google Scholar]
  13. Najiha, M.S.; Rahman, M.M.; Kadirgama, K. Performance of water-based TiO2nanofluid during the minimum quantity lubrication machining of aluminium alloy AA6061-T6. J. Clean. Prod. 2016, 135, 1623–1636. [Google Scholar] [CrossRef]
  14. Chetan; Behera, B.C.; Ghosh, S.; Rao, P.V. Application of nanofluids during minimum quantity lubrication: A case study in turning process. Tribol. Int. 2016, 101, 234–246. [Google Scholar]
  15. Jung, S.N.; Hoon, D.K.; Chung, H.; Lee, S.W. Optimization of environmentally benign micro-drilling process with nanofluid minimum quantity lubrication using response surface methodology and genetic algorithm. J. Clean. Prod. 2015, 102, 428–436. [Google Scholar]
  16. Xia, W.Z.; Zhao, J.W.; Wu, H.S.; Jiao, H.; Zhao, X.M.; Zhang, X.M.; Jiang, Z.Y. A novel nano-TiO2 additive oil-in-water lubricant for hot steel rolling. Mater. Sci. Forum 2016, 861, 201–206. [Google Scholar] [CrossRef]
  17. Zhu, Z.X.; Sun, J.L.; Wei, H.R.; Niu, T.L.; Zhu, Z.L. Research on lubrication behaviors of nano-TiO2 in water-based hot rolling liquid. Adv. Mater. Res. 2013, 643, 139–143. [Google Scholar] [CrossRef]
  18. Okeke, G.; Hammond, R.B.; Antony, S.J. Effects of heat treatment on the atomic structure and surface energy of rutile and anatase TiO2 nanoparticles under vacuum and water environments. Chem. Eng. Sci. 2016, 146, 144–158. [Google Scholar] [CrossRef]
  19. Nicholas, T.N.; Michael, K.S.; Steven, J.H.; Linda, F.H.; Suresh, C.P. A systematic study of the effect of silver on the chelation of formic acid to a titanium precursor and the resulting effect on the anatase to rutile transformation of TiO2. J. Phys. Chem. 2010, 114, 13026–13034. [Google Scholar]
  20. Eleana, K.; Vassileios, D.; Tiverios, V.; Kyriakos, B.; Alexis, L.; Christos, K. Comparative study of phase transition and textural changes upon calcination of two commercial titania samples: A pure anatase and a mixed anatase-rutil. J. Solid State Chem. 2015, 232, 42–49. [Google Scholar]
  21. Cheng, L.W.; Weng, S.H.; Hsueh, L.C.; Huey, J.L.; Horng, H.K.; Moo, C.W. Kinetics of anatase transition to rutile TiO2 from titanium dioxide precursor powders synthesized by a sol-gel process. Ceram. Int. 2016, 42, 13136–13143. [Google Scholar]
  22. Sajad, Z.; Reza, J.N.; Masoud, A. The sources of the micro stress and strain inhomogeneity in dual phase steels. Mater. Sci. Eng. A 2016, 674, 384–396. [Google Scholar]
  23. Ingole, S.; Charanpahari, A.; Kakade, A.; Umare, S.S.; Bhatt, D.V.; Menghani, J. Tribological behavior of nano TiO2 as an additive in base oil. Wear 2013, 301, 776–785. [Google Scholar] [CrossRef]
  24. Kumara, P.; Banerjee, M.K.; Hodgson, P.; Choudhray, A.R. Warm working characterization of low carbon steel in hot rolling. Mater. Today Proc. 2017, 4, 9505–9508. [Google Scholar] [CrossRef]
  25. Dwivedi, D.K. Adhesive wear behaviour of cast aluminium–silicon alloys: Overview. Mater. Des. 2010, 31, 2517–2531. [Google Scholar] [CrossRef]
  26. Zhang, C.; Wu, R.; Song, C.; Zhang, Y.F.; Li, S.L.; Tan, J.M. The grain refining and strengthening mechanism of C-Mn steel by CSP. Adv. Mater. Res. 2011, 1278, 261–263. [Google Scholar] [CrossRef]
  27. Hong, Y.S.; Hai, T.L.; Hui, H.L.; Hao, Z.L.; Wen, Q.L.; Xiao, M.Z.; Guo, D.W. Effect of hot rolling reduction on microstructure, texture and ductility of strip-cast grain-oriented silicon steel with different solidification structures. Mater. Sci. Eng. A 2014, 605, 260–269. [Google Scholar]
  28. Ouyang, W.Y.; Kuna, E.; Yepez, A.; Balu, A.M.; Romero, A.A.; Colmenares, J.C.; Luque, R. Mechanochemical synthesis of TiO2nanocompositesas photocatalysts for benzyl alcohol photo-oxidation. Nanomaterials 2016, 6, 93. [Google Scholar] [CrossRef] [PubMed]
Figure 1. Schematic of the four-ball rolling friction.
Figure 1. Schematic of the four-ball rolling friction.
Nanomaterials 08 00111 g001
Figure 2. Sketches of (a) hot rolling and (b) lubrication during hot rolling.
Figure 2. Sketches of (a) hot rolling and (b) lubrication during hot rolling.
Nanomaterials 08 00111 g002
Figure 3. Friction coefficient-time curves of traditional lubricating fluid and nano-TiO2 fluid.
Figure 3. Friction coefficient-time curves of traditional lubricating fluid and nano-TiO2 fluid.
Nanomaterials 08 00111 g003
Figure 4. Optical micrograph and 3D topography of hot-rolled surface lubricated with (a) non-lubricant; (b) traditional lubricating fluid and (c) nano-TiO2lubricating fluid.
Figure 4. Optical micrograph and 3D topography of hot-rolled surface lubricated with (a) non-lubricant; (b) traditional lubricating fluid and (c) nano-TiO2lubricating fluid.
Nanomaterials 08 00111 g004
Figure 5. SEM images of hot-rolled surfaces lubricated with (a) non-lubricant; (b) traditional lubricating fluid and (c) nano-TiO2 fluid.
Figure 5. SEM images of hot-rolled surfaces lubricated with (a) non-lubricant; (b) traditional lubricating fluid and (c) nano-TiO2 fluid.
Nanomaterials 08 00111 g005aNanomaterials 08 00111 g005b
Figure 6. Energy dispersive spectrometry (EDS) spectra of strip surface lubricated with traditional lubricating fluid.
Figure 6. Energy dispersive spectrometry (EDS) spectra of strip surface lubricated with traditional lubricating fluid.
Nanomaterials 08 00111 g006
Figure 7. SEM images and EDS spectra of oxide scales of hot-rolled strips lubricated with (a) non-lubricant; (b) traditional lubricating fluid and (c) nano-TiO2 fluid.
Figure 7. SEM images and EDS spectra of oxide scales of hot-rolled strips lubricated with (a) non-lubricant; (b) traditional lubricating fluid and (c) nano-TiO2 fluid.
Nanomaterials 08 00111 g007
Figure 8. XPS spectra of Fe 2p, O 1s and Ti 2p on the oxide scales surface lubricated with nano-TiO2 fluid.
Figure 8. XPS spectra of Fe 2p, O 1s and Ti 2p on the oxide scales surface lubricated with nano-TiO2 fluid.
Nanomaterials 08 00111 g008
Figure 9. Microstructures of rolled strips for (a) non-lubricant; (b) traditional lubricating fluid and (c) nano-TiO2lubricating fluid.
Figure 9. Microstructures of rolled strips for (a) non-lubricant; (b) traditional lubricating fluid and (c) nano-TiO2lubricating fluid.
Nanomaterials 08 00111 g009
Figure 10. The crystal structures of (a) anatase nano-TiO2 (b) rutile nano-TiO2 (c) Fe2O3 and (d) FeO.
Figure 10. The crystal structures of (a) anatase nano-TiO2 (b) rutile nano-TiO2 (c) Fe2O3 and (d) FeO.
Nanomaterials 08 00111 g010
Table 1. Main additives of the nano-TiO2 lubricating fluid.
Table 1. Main additives of the nano-TiO2 lubricating fluid.
AdditiveContent (%)
anatase nano-TiO20.50–1.50
Glycerin4.00–8.00
triethanolamine (TEA)2.00–5.00
sodium polyacrylate (PAAS)0.02–0.08
sodium hexametaphosphate (SHMP)0.20–0.60
sodium dodecyl benzene sulfonate (SDBS)0.50–1.00
Table 2. The chemical compositions of the steel strips.
Table 2. The chemical compositions of the steel strips.
ElementCSiMnSPCrNiCu
Content (wt %)0.200.351.400.0450.0450.0300.0300.030
Table 3. Tribology performances of traditional lubricating fluid and nano-TiO2 fluid.
Table 3. Tribology performances of traditional lubricating fluid and nano-TiO2 fluid.
ConditionPB/NFriction CoefficientWear Scar Diameter/mm
1#2#3#Mean Value
traditional lubricating fluid3920.15191.1821.1791.1381.166
nano-TiO2 lubricating fluid6370.10060.6450.5800.6130.613
Table 4. The average diameters of the grains.
Table 4. The average diameters of the grains.
ConditionAverage Diameters/μm
non-lubricant18.51
traditional lubricating fluid13.86
nano-TiO2 lubricating fluid7.46
Table 5. The finishing thicknesses and spring-backs of the hot rolled steel strips.
Table 5. The finishing thicknesses and spring-backs of the hot rolled steel strips.
ConditionFinishing Thickness/mmSpring-Back/%Overall Reduction/%
non-lubricant4.9824.5083.4
traditional lubricating fluid4.5714.2584.8
nano-TiO2 lubricating fluid4.133.2586.2

Share and Cite

MDPI and ACS Style

Meng, Y.; Sun, J.; Wu, P.; Dong, C.; Yan, X. The Role of Nano-TiO2 Lubricating Fluid on the Hot Rolled Surface and Metallographic Structure of SS41 Steel. Nanomaterials 2018, 8, 111. https://doi.org/10.3390/nano8020111

AMA Style

Meng Y, Sun J, Wu P, Dong C, Yan X. The Role of Nano-TiO2 Lubricating Fluid on the Hot Rolled Surface and Metallographic Structure of SS41 Steel. Nanomaterials. 2018; 8(2):111. https://doi.org/10.3390/nano8020111

Chicago/Turabian Style

Meng, Yanan, Jianlin Sun, Ping Wu, Chang Dong, and Xudong Yan. 2018. "The Role of Nano-TiO2 Lubricating Fluid on the Hot Rolled Surface and Metallographic Structure of SS41 Steel" Nanomaterials 8, no. 2: 111. https://doi.org/10.3390/nano8020111

APA Style

Meng, Y., Sun, J., Wu, P., Dong, C., & Yan, X. (2018). The Role of Nano-TiO2 Lubricating Fluid on the Hot Rolled Surface and Metallographic Structure of SS41 Steel. Nanomaterials, 8(2), 111. https://doi.org/10.3390/nano8020111

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop