Next Article in Journal
Tailoring Characteristics of PEDOT:PSS Coated on Glass and Plastics by Ultrasonic Substrate Vibration Post Treatment
Next Article in Special Issue
A Novel Electrolytic Plasma Spraying Preparation SiO2/SiC Coating on Carbon Fiber Fabric
Previous Article in Journal
A Study on the Suitability of Mechanical Soft-Abrasive Blasting Methods to Extract Graffiti Paints on Ornamental Stones
Previous Article in Special Issue
Bioceramic Layers with Antifungal Properties
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Finite Element Simulation of Temperature and Stress Field for Laser Cladded Nickel-Based Amorphous Composite Coatings

1
School of Materials Science and Engineering, Jiangsu University of Science and Technology, Zhenjiang 212003, Jiangsu, China
2
Department of Engineering, Lancaster University, Lancaster LA1 4YW, UK
*
Author to whom correspondence should be addressed.
Coatings 2018, 8(10), 336; https://doi.org/10.3390/coatings8100336
Submission received: 24 July 2018 / Revised: 18 September 2018 / Accepted: 19 September 2018 / Published: 24 September 2018

Abstract

:
In this paper, a nickel-based amorphous composite coating was obtained on the carbon steel surface by the laser cladding process. The thermal field and stress distribution were simulated by using ANSYS finite element software where the moving heat source and powder feeding were modelled by the “Element birth and death” method. The simulation results were verified by comparing the cross-sectional profile of fusion lines and X-ray stress measurements, respectively. The results on thermal field showed that the cooling rate of the coating could reach up to 10389.15 K/s and it gradually decreased from the outside surface to the interior, which promoted the formation of amorphous phase. The simulated stress field showed that the coating was in the state of tensile stress after cladding and the longitudinal stress was larger than the transverse stress. The coating was experienced with tensile plastic deformation along the laser scanning direction, which resulted in longitudinal residual stress. A higher stress concentration was occurred between the coating layer and substrate, which increased the susceptibility of crack formation. The test results on transverse residual stress were generally consistent with the simulation. On the contrary, the measured longitudinal stress was nearly close to zero, which was not in agreement with the model due to the formation of cracks.

1. Introduction

Amorphous alloy, which is also known as metallic glass, is a type of metallic material that is disordered in long-range, but ordered in short-range at the atomic level. The particularity of its atomic arrangement differs the performance of amorphous alloy from the traditional crystalline alloyed materials. When compared with the crystalline alloy with same composition, amorphous alloy exhibits excellent physical, chemical, and mechanical properties [1,2,3]. However, the high cost and difficulties in producing large dimensioned amorphous alloy restrict its wider applications in industry [4,5]. With the help of laser processing technology, the preparation of amorphous coating on the surface of traditional crystalline materials is an effective and feasible way to overcome the limitation of shape and size, reduce the material cost, and expand the application fields [6,7]. Amorphous coating can be obtained by applying a high power laser beam, with or without additional feeding material, on the surface of crystalline substrate at a very fast scanning speed, so that a thin layer of material is melted and cooled down at a very high rate. When certain metallurgical conditions are met, amorphous coating will be formed on the surface of crystalline substrate. Amorphous coating often exhibits high microhardness, excellent corrosion resistance and wearing resistance, and it also presents extensive potential industrial applications, such as in nuclear energy, thermal power, chemical plant, shipping, and sewage disposal systems, etc. [8].
In order to obtain amorphous coating, the cooling rate of the molten material needs to reach a critical value as per specific alloy [9]. However, during the laser remelting/cladding process, the laser scanning speed is very fast, so that it is difficult to measure the temperature change through traditional thermocouple or infrared thermometer [10,11]. Meanwhile, due to the uneven heating and cooling, the amorphous coating that was prepared by laser surface processing technology has a high residual stress peak with gradient distribution characteristic. Accordingly, it is difficult to accurately measure the stress distribution.
On the basis of significant advancement of modern computing technology, numerical simulation has showed its great potential to solve these problems. The studies on the numerical simulation of laser cladding process have been reported in recent years and the results have demonstrated that numerical simulation is an effective tool for predicting the thermal behavior of materials during the laser cladding process. Parisa Farahmand et al. developed a three-dimensional (3D) transient uncoupled thermo-elastic-plastic model to simulate the thermal process and thermally induced residual stress in the laser cladding process. The numerical and experimental results indicated that the model accurately predicted the characteristics of the laser cladding process [12]. Youxiang Chew et al. conducted the thermal and mechanical analyses for the laser cladding of single clad and double adjacent clads while using the finite element method. The numerical results of the thermal and residual stress field were compared with heat affected zone (HAZ) profiles on the cross sectional view and X-ray diffraction (XRD) stress measurements, respectively [13]. Recently, the element birth and death method was introduced to simulate the powder feeding for the laser cladding process, in which the elements for the clad were “killed” before cladding by multiplying their stiffness by a severe reduction factor, and thus equivalently deactivating their load, mass, and specific heat. Those elements were reactivated with the scanning speed afterwards. It was concluded that the element birth and death method presented a higher accuracy [14,15].
In this paper, nickel based amorphous coating was prepared by laser cladding process. The temperature field distribution was simulated while using “element birth and death” method in ANSYS finite element software (16.0, Ansys, Inc., Berkeley, CA, USA), and the stress field distribution was then obtained by the indirect method. The temperature and the stress fields were verified by comparing cross-sectional profile and X-ray stress measurement, respectively.

2. Materials and Methods

The (Ni0.6Fe0.4)65B18Si10Nb4C3 (at.%) alloy powders that were used in this study were obtained by high pressure argon atomization. The macroscopic appearance of the powder and its X-ray diffraction (XRD, Shimadzu Corporation, Kyoto, Japan) pattern are shown in Figure 1. As shown in Figure 1a, the powder granules are very uniform with spherical shape. The powder diameter is in the range of 50–75 μm, which ensures the fluency of powder transmission during cladding process. As shown in Figure 1b, the XRD spectrum of the powder shows a widened diffuse scattering peak around 44° with some faint crystal peaks embedded, indicating that the Ni-Fe-B-Si-Nb-C alloy powder that was used in the cladding is mainly amorphous and contains very few crystalline phases. The base material used in this research is AISI 1045 steel with a hardness of ~200 HV and its chemical compositions is shown in Table 1.
Before laser cladding experiment, the powder was dried at 200 °C to remove moisture. The cladding scanning speed and power of laser were 64 mm/s and 3600 W, respectively. The feeding rate of powder was 19 g/min. The distance between laser cladding nozzle and substrate surface was 15 mm. After laser cladding, the composition of the central phase of the coating was analyzed by XRD (40 kV, Cu Kα radiation, scanning range 20°–90°, scanning speed 4°/min, step size 0.02°). The microstructure of the coating was observed by scanning electron microscopy (SEM, Carl Zeiss Microscopy GmbH, Jena, Germany).
X-350A X-ray stress tester (Aster Stress Technology Co., Ltd., Handan, Hebei, China) was used to measure the residual stress of the clad and substrate. The test positions are distributed as shown in Figure 2. Lx was the test area along the path perpendicular to the laser cladding scan direction. The starting point was 0.5 mm away from the center axis, and the test points were separated by 1 mm for longitudinal and transverse residual stress measurement.

3. Microstructure and Phase Composition of Coating

Figure 3a shows the morphology of the laser cladded coating on the cross-sectional view. The thickness of the coating is about 0.2 mm. The fusion line between the coating and the substrate is relatively stable and no obvious dilution can be observed. There is also a crack formed in the coating. Figure 3b shows the microstructure within the white dotted rectangle in Figure 3a. The microstructure can be divided into three regions: coating, coating/substrate fusion zone, and the substrate. There exists different microstructure in different regions of coating. They are columnar dendrites (Layer I), amorphous phase + NbC particles (Layer II), and fine dendrites + NbC particles (Layer III).
Figure 4 shows the XRD spectrum of the laser cladded coating. An amorphous diffuse peak and few sharp crystal diffraction peaks were produced near the 44° (2θ) angle. The crystal peaks were identified as γ(Fe, Ni), Fe2B, and NbC phases, respectively, after retrieving the standard PDF card. To calculate the volume fraction from XRD results (Figure 4), the integrated areas of the amorphous and crystalline peaks were separated while using computer software and the Vf of amorphous phase was calculated while using the following equation [16]:
V f = A a m o r A a m o r + A c r y s t
where Vf is the volume fraction of amorphous phase in the coating formed by laser cladding process. Aamor and Acryst are the total integrated area corresponding to crystalline and amorphous phases, respectively [16]. The results showed that the volume fraction of amorphous phase in the middle of the coating was about 66.9%.

4. Finite Element Simulation

Finite element model of the laser cladded coating was established in the ANSYS software preprocessing module (/PREP7). Because the coating is very thin and the angle between the coating and the coating/substrate interface is very small, it is difficult to mesh and obtain an accurate simulation result. Then, the trapezoidal model was used instead of the original size. Due to the higher temperature and stress gradient in and near the coating, the elements in the model were arranged while using the mapping and non-uniform mesh as shown in Figure 5. The thermal properties of the substrate and the cladding alloys are obtained from the reference [10]. The latent heat of fusion 60.73 kJ/kg was used to assume the solid/liquid phase transformation. The mechanical properties used for residual stress simulation are given in Table 2 and Table 3. In this paper, the element birth and death method was used to simulate the temperature field.
The governing equation of heat conduction in Cartesian coordinates is given by:
ρ c T t = k ( 2 T x 2 + 2 T y 2 + 2 T z 2 ) + Q
where x, y, and z are Cartesian coordinates, k is thermal conductivity, c is specific heat, Q is surface heat flux, T is temperature, and t is time. A surface heat flux (Q) in Gaussian distribution was applied on the coating, and the distribution of the heat flux is described, as follows:
Q = 2 η P π R 2 exp ( 2 r 2 R 2 )
where η is heat transfer efficiency (η = 0.85), P is laser power (P = 3600 W), R is beam radius (R = 2.5 mm), and r is the distance from the center of the laser beam. At the boundaries, the heat losses from the plate surfaces to the surroundings took place by means of natural convection and radiation effects. In this study, the radiation effects were ignored and the convection coefficients at different degrees are shown in Figure 6.
Mechanical (stress) simulation is based on the thermo-elastic–plastic model. The nonlinear analysis of residual stress in the laser cladding process is based on the strains that are generated from expansion and contraction due to the thermal gradient, elastic effects, plastic strains, volumetric changes, and transformation plasticity. The total generated strains can be expressed, as follows:
Δ ε i j t o t = Δ ε i j e + Δ ε i j t h + Δ ε i j p + Δ ε i j T r p + Δ ε i j Δ V
where Δ ε i j e is the elastic strain increment, Δ ε i j t h is the thermal strain increment, Δ ε i j p is the plastic strain increment, Δ ε i j T r p is the phase transformation strain increment, and Δ ε i j Δ V is the volumetric strain increment. As for boundary conditions, the substrate was assumed to be stress free at the beginning of the process. To simulate the clamping effect on the substrate, the nodes on the bottom surface of the substrate were constrained to zero vertical displacement.
Figure 7 shows the distribution on temperature fields at different time moments. At the beginning (0.125 s), the higher temperature was located under the laser heat source and the peak temperature was about 3567 °C. With continuous movement of the heat source, the tail of the isothermal line was elongated to form an oval shape, and the peak temperature increased. In the initial stage of laser cladding, the peak temperature had a rapid rise period and it then was stabilized quickly. With the loading heat source moving forward, the laser heat input in the cladding process was basically balanced with the convection heat dissipation from the substrate surface and the elongated oval temperature field contour was basically stable. The temperature field in this state was called as quasi-steady-state temperature field. The laser cladding temperature field and the laser heat source moved forward at the same speed. Figure 7d shows the temperature distribution under 1800 s of atmosphere cooling after laser cladding. The temperature of the substrate in each region was basically the same to about 31 °C, the room temperature.
When the laser cladding time was 2 s, the temperature field was in a quasi-steady state. The cross-sectional temperature distribution of the coating perpendicular to the laser scanning direction is shown in Figure 8. As the heat source firstly acted on the coating surface, the top surface of the coating had the highest temperature. The thermal conductivity of the substrate resulted in the temperature profile to decrease with the coating penetrated into the substrate. As shown in Figure 9, the region in red color is higher than the melting point of 1491 °C, which indicates that the red color region was melted during the laser cladding process. The comparison between the experimental result and temperature field indicates that the temperature that was predicted by the developed model is in good agreement with the simulated results.
Figure 10 shows the thermal cycling curves of the laser cladded coating at different depths from surface. As the depth from the coating surface increases, the heating rate and the peak temperature decrease. At the top of the coating, the peak temperature is 3455.41 °C. With the increase of the depth from the surface, the peak temperature decreases. As the distance from the coating surface continues to increase, the peak temperature at the depth of 940 μm is only 897.14 °C, which is obviously lower than the melting temperature of the substrate, but higher than the martensitic transformation temperature, where the substrate will not melt. Martensitic transformation is occurred, where it belongs to the heat affected zone.
In order to obtain the heating and cooling rate at different depths of the coating, derivation calculus of Figure 10 was conducted, and the results are shown in Figure 11. It can be seen that during the laser cladding process, the heating rate was higher than the cooling rate throughout the coating. The heating rate and cooling rate were between 6620.25–13669.2052 K/s and 3547.84–10389.15 K/s, which are much larger than the critical cooling rate (49.3 K/s) for the amorphous formation of this alloy system. In the formation of amorphous coating, the cooling rate is one of the most important factors. The cooling rate at different layer may also change the amorphous forming ability of the laser cladded coating. The results showed that the cooling rate decreased with the increase of the depth. In other words, the cooling rate reduced sequentially from layer I, layer II, to layer III in Figure 3. In layer II, the alloy composition and cooling rate were both beneficial to the formation of amorphous phase. While, in layer I and layer III, some crystalline phase were formed. This is mainly due to the existence of heterogeneous nucleation in these two layers [17,18].
Figure 12 shows the distribution of von Mises, longitudinal stress, and transverse stress along path Lx. It can be seen that from the middle of the coating to the edge of the substrate, the von Mises of the substrate surface increased firstly and then decreased sharply, as shown in Figure 11a. The coating was subjected to a maximum von Mises stress of 354 MPa at the coating/substrate interface. The high stress distribution at the clad/substrate interface was likely caused by the sudden change in width across the interface and the big difference in thermal properties of the laser cladded coating and the substrate [19]. When the distance from the coating was larger than 1 mm, the stress was almost 0. Thus, the stress of the laser cladded coating was mainly concentrated in the coating area. The longitudinal and transverse stress distribution of the coating had the same distribution characteristics as the von Mises, although the longitudinal stress of the coating was greater than the transverse stress. This is mainly due to that the width of the laser cladded coating was only 0.45 mm, and accordingly, the resistance to deformation in the transverse direction was limited. While in the longitudinal direction, the length of the coating increased along with the laser cladding process, and the resistance to deformation was accumulated, which resulted in a higher residual stress in this direction.
The tested results on longitudinal and transverse residual stress while using the X-ray diffraction method along the path Lx are shown in Figure 13. It can be seen that the longitudinal residual stress parallel to the laser scanning direction was almost consistent with the stress in the coating and the substrate, both of which were close to 0 MPa. For the transverse residual stress perpendicular to the laser scanning direction, the coating was subjected to a large tensile stress value of 756 MPa, and then decreased sharply. The compressive residual stress was presented in the substrate, especially in HAZ. The transverse tensile stress of the coating was similar to the numerical simulation results of residual stress. However, the longitudinal tensile stress of the measured coating differed greatly from the numerical simulation results. The reason is that the crack initiation and cracks in the coating were not considered in the numerical simulation. However, in the actual laser cladding process, the cracks were always formed in the coating and the stress may be relaxed. In this study, the width of the laser cladded coating was only 0.45 mm, so the resistance to deformation in the transverse direction was limited. While in the longitudinal direction, the length of the coating increased along with the laser cladding process, the resistance to deformation was accumulated, which led to a higher residual stress in this direction. So the cracks were always formed perpendicular to the laser cladding direction, as seen in Figure 14. Therefore, the measured stress values were relatively lower. It is easy to obtain a conclusion that the residual tensile stress along the laser scanning direction was relatively larger and there was a maximum at the edge of the coating, which induced the cracks that were formed perpendicular to the laser scanning direction at the edge of the coating.

5. Conclusions

  • Using the coaxial powder feeding laser cladding method, three layers consisting of columnar dendrites, amorphous phase, and NbC particles and fine dendrites and NbC particles were formed in the laser cladded nickel based coating. The XRD results showed that the volume fraction of amorphous phase in the middle of the coating is about 66.9%.
  • Numerical simulation results showed that the peak temperature was 3455.41 °C at the top surface of the coating. With the increase of the depth from the top surface, the peak temperature decreased. The heating rate and the cooling rate were between 6620.25–13669.2052 K/s and 3547.84–10389.15 K/s.
  • The von Mises stress reached the maximum near the coating edge and then dropped rapidly. Residual stress was disappeared at 1 mm from the coating edge. The longitudinal stress of the laser cladded coating was lower than the transverse stress, which resulted from cracks formation during the single pass laser cladding process.

Author Contributions

Software, R.L., Y.Q. and Q.Z.; Investigation, Y.T. and S.C.; Data Curation, Y.T. and S.C.; Writing-Original Draft Preparation, R.L., Q.Z. and Y.Q.; Writing-Review & Editing, Y.T.; Supervision, R.L.; Project Administration, R.L.; Funding Acquisition, B.L. and R.L.

Funding

This research was funded by the National Natural Science Foundation of China (Nos. 51775254 & 51405206) and the China Postdoctoral Science Foundation (No. 2017M611750).

Conflicts of Interest

There is no potential conflict of interest.

References

  1. Wang, W.H.; Dong, C.; Shek, C.H. Bulk metallic glasses. Mater. Sci. Eng. R 2004, 44, 45–89. [Google Scholar] [CrossRef]
  2. Kwon, D.H.; Lee, K.M.; Park, E.S.; Kim, H.J.; Bae, J.C.; Huh, M.Y. Wear behaviors of bulk metallic glass alloy and hardened steel having the same hardness value. J. Alloys Compd. 2012, 536S, S99–S102. [Google Scholar] [CrossRef]
  3. Geng, Y.; Wang, Y.; Wang, Z.; Qiang, J.; Wang, H.; Dong, C.; Tegus, O. Formation and structure-property correlation of new bulk Fe-B-Si-Hf metallic glasses. Mater. Des. 2016, 106, 69–73. [Google Scholar] [CrossRef]
  4. Nishiyama, N.; Takenaka, K.; Miura, H.; Saidoh, N.; Zeng, Y.; Inoue, A. The world’s biggest glassy alloy ever made. Intermetallics 2012, 30, 19–24. [Google Scholar] [CrossRef]
  5. Inoue, A.; Takeuchi, A. Recent development and application products of bulk glassy alloys. Acta Mater. 2011, 59, 2243–2267. [Google Scholar] [CrossRef]
  6. Mojaver, R.; Mojtahedi, F.; Shahverdi, H.R.; Torkamany, M.J. Study on feasibility of producing an amorphous surface layer of Fe49Cr18Mo7B16C4Nb3 by pulsed Nd:YAG laser surface melting. Appl. Surf. Sci. 2013, 264, 176–183. [Google Scholar] [CrossRef]
  7. Shu, F.; Tian, Z.; Zhao, H.; He, W.; Sui, S.; Liu, B. Synthesis of amorphous coating by laser cladding multi-layer Co-based self-fluxed alloy powder. Mater. Lett. 2016, 176, 306–309. [Google Scholar]
  8. Wang, S.L.; Zhang, Z.Y.; Gong, Y.B.; Nie, G.M. Microstructures and corrosion resistance of Fe-based amorphous/nanocrystalline coating fabricated by laser cladding. J. Alloy. Compd. 2017, 728, 1116–1123. [Google Scholar] [CrossRef]
  9. Waseda, Y.; Chen, Ho.; Jacob, K.T.; Shibata, H. On the glass forming ability of liquid alloys. Sci. Technol. Adv. Mater. 2008, 9, 023003. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  10. Li, R.; Jin, Y.; Li, Z.; Zhu, Y.; Wu, M. Effect of the remelting scanning speed on the amorphous forming ability of Ni-based alloy using laser cladding plus a laser remelting process. Surf. Coat. Technol. 2014, 259, 725–731. [Google Scholar] [CrossRef]
  11. Zhu, Y.; Li, Z.; Li, R.; Li, M.; Feng, K.; Wu, Y. High power diode laser cladding of Fe–Co–B–Si–C–Nb amorphous coating: Layered microstructure and properties. Surf. Coat. Technol. 2013, 235, 699–705. [Google Scholar] [CrossRef]
  12. Farahmand, P.; Kovacevic, R. An experimental–numerical investigation of heat distribution and stress field in single-and multi-track lase rcladding by a high-power direct diode laser. Opt. Laser Technol. 2014, 63, 154–168. [Google Scholar] [CrossRef]
  13. Chew, Y.; Pang, J.H.L.; Bi, G.; Song, B. Thermo-mechanical model for simulating laser cladding induced residual stresses with single and multiple clad beads. J. Mater. Process. Technol. 2015, 224, 89–101. [Google Scholar] [CrossRef]
  14. Hao, M.; Sun, Y. A FEM model for simulating temperature field in coaxial laser cladding of Ti6Al4V alloy using an inverse modeling approach. Int. J. Heat Mass Transf. 2013, 64, 352–360. [Google Scholar] [CrossRef]
  15. Yong, Y.; Fu, W.; Deng, Q.; Chen, D. A comparative study of vision detection and numerical simulation for laser cladding of nickel-based alloy. J. Manuf. Process. 2017, 28, 364–372. [Google Scholar] [CrossRef]
  16. Yang, H.W.; Wea, J.; Quan, M.X.; Wang, J.Q. Evaluation of the volume fraction of nanocrystals devitrified in Al-based amorphous alloys. J. Non-Cryst. Solids 2009, 355, 235–238. [Google Scholar] [CrossRef]
  17. Chen, S.; Li, R.; Zheng, Q.; Li, Z. Layered microstructure distribution and forming mechanism of laser-processed Ni-Fe-B-Si-Nb-C amorphous composite coatings. Mater. Trans. 2016, 57, 1807–1810. [Google Scholar] [CrossRef]
  18. Katakam, S.; Kumar, V.; Santhanakrishnan, S.; Rajamure, R.; Samimi, P.; Dahotre, N.B. Laser assisted Fe-based bulk amorphous coating: Thermal effects and corrosion. J. Alloy. Compd. 2014, 604, 266–272. [Google Scholar] [CrossRef]
  19. Finnie, S.; Cheng, W.; Finnie, I.; Drezet, J.M.; Gremaud, M. The computation and measurement of residual stresses in laser deposited layers. Trans. ASME 2003, 125, 302–308. [Google Scholar] [CrossRef]
Figure 1. Scanning electron microscopy (SEM) morphology and the X-ray diffraction (XRD) spectrum of the powder: (a) Macroscopic appearance; (b) XRD.
Figure 1. Scanning electron microscopy (SEM) morphology and the X-ray diffraction (XRD) spectrum of the powder: (a) Macroscopic appearance; (b) XRD.
Coatings 08 00336 g001
Figure 2. Schematic diagram of residual stress test positions (mm).
Figure 2. Schematic diagram of residual stress test positions (mm).
Coatings 08 00336 g002
Figure 3. Cross-sectional morphology and microstructure of the laser cladded coating: (a) Cross-section morphology; (b) Microstructure.
Figure 3. Cross-sectional morphology and microstructure of the laser cladded coating: (a) Cross-section morphology; (b) Microstructure.
Coatings 08 00336 g003
Figure 4. XRD spectrum of laser cladding coating.
Figure 4. XRD spectrum of laser cladding coating.
Coatings 08 00336 g004
Figure 5. Geometry model (a) and meshing (b) of laser cladded coating.
Figure 5. Geometry model (a) and meshing (b) of laser cladded coating.
Coatings 08 00336 g005
Figure 6. Convection coefficient between the boundary and the surroundings.
Figure 6. Convection coefficient between the boundary and the surroundings.
Coatings 08 00336 g006
Figure 7. Temperature field of the laser cladded coating at different time. (a) t = 0.125 s; (b) t = 0.500 s; (c) t = 2.000 s; and, (d) t = 1806.00 s.
Figure 7. Temperature field of the laser cladded coating at different time. (a) t = 0.125 s; (b) t = 0.500 s; (c) t = 2.000 s; and, (d) t = 1806.00 s.
Coatings 08 00336 g007
Figure 8. Temperature field of coating cross section (t = 2 s).
Figure 8. Temperature field of coating cross section (t = 2 s).
Coatings 08 00336 g008
Figure 9. Comparison between experiment result and simulated temperature field (°C).
Figure 9. Comparison between experiment result and simulated temperature field (°C).
Coatings 08 00336 g009
Figure 10. Thermal cycling curve of coating at different depths from surface.
Figure 10. Thermal cycling curve of coating at different depths from surface.
Coatings 08 00336 g010
Figure 11. Heating and cooling rates during the laser cladding process.
Figure 11. Heating and cooling rates during the laser cladding process.
Coatings 08 00336 g011
Figure 12. Simulated residual stress of coating along the path Lx. (a) Von Misses; and, (b) Longitudinal and transverse residual stress.
Figure 12. Simulated residual stress of coating along the path Lx. (a) Von Misses; and, (b) Longitudinal and transverse residual stress.
Coatings 08 00336 g012
Figure 13. Residual stress at different distances from the middle line of the coating.
Figure 13. Residual stress at different distances from the middle line of the coating.
Coatings 08 00336 g013
Figure 14. Cracks formed in the laser cladded coating.
Figure 14. Cracks formed in the laser cladded coating.
Coatings 08 00336 g014
Table 1. Chemical compositions of AISI 1045 steel substrate.
Table 1. Chemical compositions of AISI 1045 steel substrate.
ElementCSiMnCrNiCuFe
Content % (wt.%)0.42–0.500.17–0.370.50–0.800.250.300.25Balance
Table 2. Mechanical properties of the cladding alloys.
Table 2. Mechanical properties of the cladding alloys.
Temperature °C Linear Expansion %Young Modulus GPaPoisson’s Ratio
250214.3260.28018
1000.105210.7820.28156
3000.399200.7160.28528
6000.879183.8770.29088
8000.28414.5030.38329
10000.250.9040.43622
12002.080.0040.48551
15003.4390.00040.4917
20006.17200.5
300012.81500.5
500032.49700.5
Table 3. Mechanical properties of the AISI 1045 steel substrate.
Table 3. Mechanical properties of the AISI 1045 steel substrate.
Temperature °CLinear Expansion %Young Modulus GPaPoisson’s Ratio
250209.5770.28886
1000.0926206.2380.29164
3000.361192.7740.29904
6000.821158.7630.31014
8000.913128.0280.35039
10001.394108.3020.36211
12001.87988.0510.48551
15004.03200.5
20006.45900.5
300013.09400.5
500033.50600.5

Share and Cite

MDPI and ACS Style

Li, R.; Qiu, Y.; Zheng, Q.; Liu, B.; Chen, S.; Tian, Y. Finite Element Simulation of Temperature and Stress Field for Laser Cladded Nickel-Based Amorphous Composite Coatings. Coatings 2018, 8, 336. https://doi.org/10.3390/coatings8100336

AMA Style

Li R, Qiu Y, Zheng Q, Liu B, Chen S, Tian Y. Finite Element Simulation of Temperature and Stress Field for Laser Cladded Nickel-Based Amorphous Composite Coatings. Coatings. 2018; 8(10):336. https://doi.org/10.3390/coatings8100336

Chicago/Turabian Style

Li, Ruifeng, Yi Qiu, Qichi Zheng, Bin Liu, Shujin Chen, and Yingtao Tian. 2018. "Finite Element Simulation of Temperature and Stress Field for Laser Cladded Nickel-Based Amorphous Composite Coatings" Coatings 8, no. 10: 336. https://doi.org/10.3390/coatings8100336

APA Style

Li, R., Qiu, Y., Zheng, Q., Liu, B., Chen, S., & Tian, Y. (2018). Finite Element Simulation of Temperature and Stress Field for Laser Cladded Nickel-Based Amorphous Composite Coatings. Coatings, 8(10), 336. https://doi.org/10.3390/coatings8100336

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics