Next Article in Journal
Hydrogen Permeation, and Mechanical and Tribological Behavior, of CrNx Coatings Deposited at Various Bias Voltages on IN718 by Direct Current Reactive Sputtering
Next Article in Special Issue
Corrosion Resistance and Durability of Superhydrophobic Copper Surface in Corrosive NaCl Aqueous Solution
Previous Article in Journal
Application of Graphene-Oxide-Modified Polyacrylate Polymer for Controlled-Release Coated Urea
Previous Article in Special Issue
Chemical and Physical Pathways for Fabricating Flexible Superamphiphobic Surfaces with High Transparency
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

New Electrospun Polystyrene/Al2O3 Nanocomposite Superhydrophobic Coatings; Synthesis, Characterization, and Application

by
Ahmed Bahgat Radwan
1,
Aboubakr M. Abdullah
1,*,
Adel M. A. Mohamed
2,3 and
Mariam A. Al-Maadeed
1
1
Center for Advanced Materials, Qatar University, Doha 2713, Qatar
2
Département des Sciences Appliquées, Université du Québec à Chicoutimi, Chicoutimi, QC G7H 2B1, Canada
3
Department of Metallurgical and Materials Engineering, Faculty of Petroleum and Mining Engineering, Suez University, Suez 43721, Egypt
*
Author to whom correspondence should be addressed.
Coatings 2018, 8(2), 65; https://doi.org/10.3390/coatings8020065
Submission received: 20 December 2017 / Revised: 31 January 2018 / Accepted: 1 February 2018 / Published: 8 February 2018
(This article belongs to the Special Issue Superhydrophobic Coatings)

Abstract

:
The effect of electrospinning operational parameters on the morphology, surface roughness, and wettability of different compositions of electrospun polystyrene (PS)–aluminum oxide (Al2O3) nanocomposite coatings was investigated using different techniques. For example, a scanning electron microscope (SEM) coupled with an energy dispersive X-ray (EDX) unit, a Fourier transform infrared (FTIR) spectrometer, an atomic force microscope (AFM), and water contact angle (WCA), and contact angle hysteresis (CAH) measurements using the sessile droplet method, were used. The latter used 4 µL of distilled water at room temperature. PS/Al2O3 nanocomposite coatings exhibited different morphologies, such as beaded fibers and microfibers, depending on the concentration ratio between the PS and Al2O3 nanoparticles and the operational parameters of the electrospinning process. The optimum conditions to produce a nanocomposite coating with the highest roughness and superhydrophobic properties (155° ± 1.9° for WCA and 3° ± 4.2° for CAH) are 2.5 and 0.25 wt % of PS and Al2O3, respectively, 25 kV for the applied potential and 1.5 mL·h−1 for the solution flow rate at 35 °C. The corrosion resistance of the as-prepared coatings was investigated using the electrochemical impedance spectroscopy (EIS) technique. The results have revealed that the highly porous superhydrophobic nanocomposite coatings (SHCs) possess a superior corrosion resistance that is higher than the uncoated Al alloy by three orders of magnitude.

1. Introduction

Superhydrophobic surfaces with low sliding angle (SA ≤ 10°) and high water contact angle (WCA ≥ 150°) exhibit a low resistance to water mobility on the surface as a result of the embedded air in the composite under the water on these surfaces [1,2]. Such surfaces have attracted a significant interest because of their potential applications in many industrial fields and biological processes, e.g., highly corrosion resistant [3] and anti-adhesive coatings [4], self-cleaning materials [5], antifingerprint optical devices [6], printing technologies [7], water–oil separation [8], and digital microfluidics [9].
Many examples of natural superhydrophobic materials are exist, e.g., the lotus leaf, which is equipped with hierarchical surface projections, insect wings, and animal fur [10,11,12,13,14]. The superhydrophobic behavior is usually attributed to a combination of a hydrophobic surface and micro or nanostructures.
Synthetic superhydrophobic surfaces have been synthesized in the last decades in which the surface chemistry and roughness were tailored to decrease the surface energy and maintain trapped air at the material-water interface. The synthesis was achieved using different methods, e.g., microfabrication and chemical processes [15,16,17,18]. In 1943, a superhydrophobic material was fabricated using electrospinning [19], which is a technique that uses a high electric field to produce fibers from solutions of polymeric materials. The properties of these solutions, such as the surface tension, the viscosity, and the molecular weight of the polymer, in addition to the electrospinning parameters, e.g., the distance between a needle and a substrate, the solution flow rate, and the applied voltage, are the main factors that influence the electrospinning process that affects the properties of the produced fibers. Consequently, the optimum conditions of the electrospinning process for numerous polymers were studied [20,21,22,23,24]. It is worth mentioning that the advantage of the electrospinning technique compared to other ones, e.g., drawing [25] template synthesis [26], phase separation [27], and self-assembly [28], is the ability to develop it for mass production, simplicity, and inexpensiveness. In addition, it can be used for a wide range of polymers to create nanofibers [29,30,31,32].
Polystyrene (PS) is a glassy and amorphous polymer that is commonly rigid and relatively cheap. It is a poor barrier to oxygen and water vapor and has a relatively low melting point [33]. PS is currently used in several applications, e.g., packaging, electrical/electronic applications, toys, sheets, household goods, insulation, etc. It should be mentioned that selecting the solvent in the electrospinning of PS is a critical issue. A systematic analysis was conducted for eighteen various solvents to find the most suitable one for PS electrospinning. It was concluded that N,N-dimethylacetamide (DMAc) and tetrahydrofuran (THF) are the best candidates [34].
Acatay et al. studied the relationship between the surface morphology and the degree of superhydrophobicity of a material [35]. The fabrication of a superhydrophobic PS by the addition of inorganic nanomaterials such as SiO2 [36], TiO2 [37], and MnO2 [38] has been studied. The addition of these nanoparticles led to an increase in the surface roughness and a decrease in the surface energy of the PS–oxide nanoparticles composite coating in addition to enhancing the formation of hierarchical shapes [39]. Electrospun PS/Al2O3 nanocomposite is also expected to have, at least, the same superhydrophobic nature as the PS/SiO2, TiO2, or MnO2 with better physical properties, e.g., transparency and stability, insulation and hardness [40]. Furthermore, its high corrosion resistance can be exploited in many applications, e.g., protective coating, fire retarder, insulators, and catalysis [41]. Therefore, the target of this work is studying the effect of the compositional ratio between the PS and the Al2O3 nanoparticles in addition to the electrospinning operational parameters on the superhydrophobic behavior of the nanocomposite coatings on Al substrates. Moreover, the protection of the fabricated superhydrophobic coatings (SHCs) against corrosion is studied in saline water.

2. Materials and Methods

Commercial aluminum foil was used as a substrate for the experiments. PS with a molecular weight of 250 kDa was purchased from Sigma-Aldrich (Taufkirchen, Germany). DMAc and THF, obtained from BDH Chemicals (Doha, Qatar), were used as nonvolatile and volatile solvents, respectively. Al2O3 nanoparticles of a size <20 nm were used to enhance the hydrophobicity of PS based-polymer matrix (Sigma-Aldrich, Taufkirchen, Germany).
Different amounts of PS were dissolved in a mixture of 70 wt % DMAc and 30 wt % THF at 35 °C for 12 h and stirred until getting a sufficiently viscous solution that is required for electrospinning. In-parallel, different concentrations of Al2O3 nanoparticles were dispersed in DMAc/THF mixtures of the same ratio under vigorous stirring conditions until a homogenous dispersion of the nanoparticles was obtained. The dispersed Al2O3 nanoparticles in DMAc/THF were then added to the PS solution to achieve the desired weight ratio of Al2O3 to PS. The different PS and Al2O3 concentrations used in this study are shown in Table 1.
Prior to electrospinning, aluminum substrates (which will be used as a collector) were mechanically polished using Grinder polisher (Metko FORCIPO1V, Bursa, Turkey), degreased ultrasonically for 30 min, and cleaned by distilled water and finally dried. An electrospinning unit consisting of a syringe pump, a high voltage supply, and a collector was used. Syringe pump was aligned horizontally, and electric field was maintained by the high voltage power supply. The complex solutions were stored in syringes behind the needles. The distance between the tip of the needle and the collector was 15 cm. The electrospinning of the nanocomposite solutions was performed using a needle with an inside diameter of 0.25 mm at flow rates of 1.5 and 2 mL·h−1 and an applied voltage of 20 and 25 kV, while the operating temperature was kept constant at 35 °C. After the electrospinning process, nanofibers were dried overnight.

Characterization Techniques

High field emission scanning electron microscopy, HFESEM, (FEI NOVA NANOSEM 450, Hillsboro, OR, USA) coupled with an energy dispersive X-ray unit, EDX, was used to investigate the morphology of the fabricated nanocomposite coatings. For water contact angle data, a 4 µL water droplet was placed onto the different coating surfaces using OCA 35 Contact Angle Measuring System (Dataphysics Instruments, Filderstadt, Germany). The sliding angle (SA) was measured by tilting the substrate until the droplet was noticed to move and the advancing (largest) contact angle (ACA) and receding (smallest) contact angle (RCA) were recorded. The initial water contact angles were measured at 5 different locations at the surface of each specimen. Fourier transform infrared spectroscopy (FTIR) spectra were recorded in a range of 4000–400 cm−1 using PerkinElmer Spectrum 400 FTIR, PerkinElmer, Waltham, MA, USA. Atomic force microscopy (AFM) analysis was carried out using an MFP-3D, Asylum Research, Santa Barbara, CA, USA. AFM was performed using a silicon tip with a radius of 10 nm and a resonance frequency of 70 kHz besides a spring constant of 2 Nm−1 in the non-contact tapping mode in air. Electrochemical impedance spectroscopy (EIS) measurements were performed using a Gamry Reference 3000 potentiostat, Warminster, PA, USA, in 3.5 wt % NaCl solutions within a frequency range of 0.01 Hz to 100 kHz with a wave amplitude of 5 mV at 25 °C. EIS data analysis was performed using a Gamry Echem Analyst software (Version 7.06, Gamry, Warminster, PA, USA). Before running any EIS experiment, the samples were immersed in the 3.5 wt % NaCl electrolyte for 30 min.

3. Results and Discussion

3.1. Surface Morphology of the Coatings

The representative SEM micrographs of the electrospun PS with different concentrations of Al2O3 nanoparticles are shown in Figure 1 and Figure 2, respectively. Different morphologies of PS in absence and presence of Al2O3 nanoparticles including beaded fibers and free beads are obtained by varying the concentration of PS and Al2O3 and/or the operational parameters of the electrospinning process. Table 2 shows the average nanofiber diameter of the different prepared coatings before and after the addition of Al2O3 nanoparticles.
The morphologies of the pure PS polymer shown in Figure 1 reveal the formation of a beaded-fiber structure. At low applied voltages, the bead shape is spindle-like, Figure 1a,b. However, increasing the applied voltage and/or the PS concentration leads to a decrease in the number of beads and changes them to a spherical-like shape, Figure 1c,d, due to the increase of the jet stretching. The bead formation can be demonstrated by the insufficient swift stretching through the flagellation of the jet [42]. This observation is inconsistent with the previous work [34]. Moreover, at low PS concentration, the elasticity is too small to supply enough resistance to tolerate the stretching, which results from the electrostatic force, leading to the formation of a large number of beads. However, by increasing the PS concentration from 2.5 to 5 wt %, the ultrafine PS fibers are formed with a small number of beads per unit area, demonstrating that the elastic properties of PS solution are more significant at high concentrations, as shown in Figure 1d.
The SEM micrographs shown in Figure 2 display the effect of adding Al2O3 nanoparticles on the surface morphology of an electrospun PS polymer. The SEM micrographs show the formation of different sizes of beaded fibers without a significant change in the surface morphology.
Table 2 shows a significant variation in the fiber diameter as the concentrations of PS polymer and Al2O3 nanoparticles, as well as the electrospinning parameters, change. It can be observed that the increase in the applied voltage from 20 to 25 kV, while other parameters are kept constant, leads to a decrease in the average nanofiber diameters of PS1 and PS3 to 340 ± 27 and 320 ± 21 nm, respectively. Increasing the applied voltage results in a large elongation of the solution owing to the greater columbic forces in the jet, in addition to the high electric field, which leads to the formation of thinner fibers [43,44]. However, as the concentration of PS is increased from 2.5 g (PS3) to 5 g (PS4), the average nanofiber diameter is increased from 320 ± 21 to 433 ± 15 nm, respectively.
The higher the quantity of polymer chains in the solution, the easier the capability of the electrospinning jet to elongate the solution, while the solvent molecules are dispersed between the polymer chains [21,34,45]. In addition, with an increase of the wt % of PS, the increased viscoelastic force can hinder the jet segment from being stretched by the constant columbic force, yielding fibers with large diameters [34]. On the other hand, it was found that the fiber diameter of PS2 and PS3 diminished to 328 ± 29 nm and 320 ± 21 nm, respectively, by reducing the flow rate from 2 to 1.5 mL·h−1. By increasing the flow rate, the quantity of polymer flowing through the tip of the needle increases, which in turn produces thick fibers. Moreover, at very high flow rates, the polymeric jet was unsettled and tended to electrospray owing to the influence of the gravitational force.
Table 2 shows the formation of fibers with different diameters after the addition of Al2O3 nanoparticles to the solutions with different PS concentration. It worth mentioning that addition of Al2O3 nanoparticles leads to a significant decrease in the diameter of the fibers in comparison with the pure PS. However, further addition of alumina nanoparticles decreases the fiber diameter from 320 ± 21 of PS3 to 290 ± 34 nm of PA3. These results are inconsistent with a previous report [46].
Figure 3a,b shows the SEM/EDX mapping of PA1 and PA3 SHCs, which verifies the presence and the uniform dispersion of the alumina nanoparticles on the beaded fiber structure.

3.2. Wettability

The effect of changing the compositional ratio between PS and Al2O3 and the different electrospinning parameters on the wettability of the PS/Al2O3 nanocomposite is investigated. Table 3 reveals the measured values of WCA and SA for both PS and PS/Al2O3 nanocomposite coatings using the sessile droplet method at ambient temperature.
Figure 4 shows snapshots for the measured WCA after and before the addition of Al2O3 nanoparticles. The WCA of the uncoated Al substrate was around 87° ± 2.2°. However, WCAs values of the PS coatings vary with the processing parameters of electrospinning, due to the variation of the fibers diameters. The highest WCA and lowest CAH of the PS–coated materials is 147° ± 1° and 14° ± 3°, respectively, for PS3, which is formed at a flow rate of 1.5 mL·h−1 and an applied voltage of 25 kV. Nevertheless, the addition of Al2O3 nanoparticles to PS polymer improved the hydrophobicity of the nanocomposite coating. The highest WCA and lowest CAH average values are 155.2° ± 1.9° and 3° ± 4.2°, respectively, for PA3.
The static contact angle is measured according to the Wenzel and Cassie–Baxter models. The hypothesis developed by Wenzel is described in Equation (1) [47,48].
cos θ = r cos θ Y
in which r is the ratio between the true surface area and the apparent one (for a rough surface r > 1 and =1 for a smooth one). θ is the apparent macroscopic WCA and θ Y is the intrinsic contact angle for the droplet on a corresponding flat surface obtained by the Young’s equation (as defined for an ideal surface). On the other hand, Cassie-Baxter regime suggested that the water droplet is suspended on the rough surfaces and is not penetrated into the channels among the rough surface, resulting in heterogeneous structures consisting of air and solids. Therefore, the contact angle in terms of the Cassie-Baxter hypothesis is given in Equation (2) [49]:
cos θ CB = r f f 1 cos θ Y f 2
in which θ CB and θ Y represent the contact angle on the rough nanocomposite coating (PS/Al2O3) and the smooth PS surfaces, respectively. f 1 and f 2 are the area fractions of the solid and air on the surface in which f 1 + f 2 = 1 . Given that θ CB is 151° ± 2.8°, 152° ± 1.2° and 155° ± 1.9° for PA1, PA2, and PA3 nanocomposite coatings, respectively, and θ Y for the PS before addition of Al2O3 equals 141° ± 2°, 143° ± 3°, and 147° ± 1° for PS1, PS2, and PS3, respectively, then the estimated values of f2 are 0.43, 0.42, and 0.47, respectively. These calculations indicate that air occupies about 43%, 42%, and 47% of the contact regions area for the as-prepared PA1, PA2, and PA3 nanocomposite coating, respectively. This confirms that the reason behind the superhydrophobicity of the PS/Al2O3 composite coating is mainly attributed to the multiscale (hierarchical) roughness of the surface, which is induced by the micro-/nano-sized fibers or beads and the nanoparticles incorporated in the polymer solution.
CAH is an important parameter to be measured besides the WCA, as it gives information about the stickiness of the surface. The high WCA of the coating does not necessarily indicate a low CAH, due to the effect of chemical heterogeneity [50]. The CAHs of PS coatings before the addition of Al2O3 nanoparticles are 24° ± 3°, 20° ± 4°, 14° ± 3°, and 32° ± 6° for PS1, PS2, PS3, and PS4 respectively, as shown in Table 3. The increase of the nanofiber diameter at high PS concentration showed a low WCA and a high CAH for PS4. After the addition of Al2O3 nanoparticles, the CAH decreased to 7.1 ± 2.3, 5 ± 3.1, and 3 ± 4.2 for PA1, PA2, and PA3, respectively. These results reveal a low adhesion force between the prepared PS/Al2O3 nanocomposite surface and water droplets, which allows water droplets to slide easily from the substrate’s surface.
In addition to the thickness of the fiber and the electrospinning parameters, the size of the nanoparticles may have an effect on the wettability. According to Conti et al. [51], a combination of silica nanoparticles of two different sizes (70 and 100 nm) increased the WCA to 147° and lowered the WCAH to 10°. However, when the size of SiO2 nanoparticles was increased to 150 nm, the WCA was decreased drastically to 124°. On the other hand, Karapanagiotis et al. [52] used Al2O3 nanoparticles with different sizes (25, 35, and 150 nm) in their coatings, and they found that the coating wettability is independent of the size of the nanoparticles. Then, in a more recent study, they [53] found an effect for the size of the nanoparticles on the wettability of their coatings, only if the concentration of the nanoparticle is high.
Figure 5 shows the FTIR spectra of pure PS and PS/Al2O3 nanocomposite coatings at different electrospinning parameters and concentrations of PS and Al2O3. The spectra for PS before and after the addition of Al2O3 with different electrospinning parameters are very similar. No remarkable changes are observed before and after addition of Al2O3. This is probably because of the small concentration of the Al2O3 used compared with the PS amount. The FTIR of Al2O3, Figure 5a, shows a transmission band located at about 3400 cm−1 that is assigned to hydrogen–bonded –O–H of the adsorbed water, while the band at 400–1000 cm−1 can be attributed to the bending stretching band of Al–O [54]. PS/Al2O3 nanocomposite and PS show the same spectra between the 700–3100 cm−1. Bands of the IR spectrum for PS correspond to their functional groups. The observed peaks at 3000–3100 cm−1 are attributed to the aromatic C–H stretching vibration and the C–H group on the PS side chain. However, the absorbance bands at 2922 and 2854 cm−1 correspond to the C–H stretching vibration of the –CH2 and –CH groups on the main PS chain. The C–C aromatic stretch and the vibration of the aromatic ring are noticed at 1494 and 1091 cm−1, respectively. The strong peaks located at 700 and 760 cm−1 are ascribed to –CH2 rocking mode and C–H out-of-plane bend, respectively. The inorganic segment of the Al–O–Al band can be noticed at 400–800 cm−1, and its absorbance intensity increases with increasing the Al2O3 content [55]. However, it is noticed that there no new bands appear after adding Al2O3 nanoparticles to the PS, which proves that (i) Al2O3 only interacted physically with PS [56], and (ii) the electrospinning in this case does not affect the chemical structure of the polymer.
To better understand the effect of nanoparticle addition on PS, AFM is used to document the surface topography of both PS and PS/Al2O3 nanocomposite coatings. AFM images in Figure 6 and Table 4 show the 3D height and the roughness values (Ra), respectively. It is clear from Table 4 that the Ra of the prepared PS coatings before the addition of the Al2O3 nanoparticles (PS1, PS2, PS3, and PS4) are slightly close to each other. In the images a–d of Figure 6, it can be noticed that the PS surface is relatively smooth and small bumps appeared on the surface, which may happen due to the beaded fibers structure. However, after the addition of Al2O3 nanoparticles, the Ra values significantly increase as shown in Table 4 and in Images e–h in Figure 6.
The Ra values of PS1, PS2, PS3, and PS4 before the addition of the Al2O3 nanoparticles are 22 ± 2, 26 ± 4, 32 ± 3, and 17 ± 4 nm, respectively. However after the addition of the nanoparticles, the surface roughness values increases to 53 ± 3, 61 ± 4, 82 ± 2, and 27 ± 3 nm for PA1, PA2, PA3, and PA4, respectively. This explains why PA3 has the highest WCAs. The AFM measurements verified the effect of the composition ratio and the electrospinning operational parameters on the surface roughness of superhydrophobic nanocomposite coatings. Generally, Al2O3 and the combination of micro beads/nano fiber structure increase the roughness, which in turn increases the WCA in comparison with the pure PS polymer. It also can be noticed that increasing the concentration of PS or the flow rate decreases the surface roughness and consequently lowers the WCA. It is worth mentioning that lowering the operational potential from 25 to 20 kV also decreases the surface roughness and consequently lowers the WCA.

3.3. Anticorrosion Performance of the As-Prepared Nanocomposite Coatings

As a non-destructive technique, EIS is usually used to study the corrosion mechanism and the corrosion resistance of SHCs. Figure 7 and Figure 8 show the Nyquist and Bode plots of the measured EIS data, respectively. The dots are the measured data, while the solid lines are the fitted data using the electrical equivalent circuit shown in Figure 9 that has two time constants. Rpo and Rct refer to the coating pore resistance and charge transfer resistance, respectively. On the other hand, Cdl1 and Cdl2 are the double layer capacitances of the constant phase elements representing the coating/solution and metal/solution interfaces, respectively. The high-frequency intercept |Z100 kHz| refers to the solution resistance (Rs), and the low-frequency intercept |Z0.01 Hz| represents the sum of the solution and charge transfer resistances. Simply, the larger the diameter of the semicircle (charge transfer resistance), the lower the corrosion rate is. Table 5 exhibits the fitted data that were attained from Gamry Echem Analyst software. The capacitances are substituted by constant phase elements (Cdl1 and Cdl2) to give a more precise fit to the experimental outcomes. The exponent (0 ≤ n ≤ 1) represents deviation from an ideal dielectric behavior; if n = 0, it shows an ideal resistor, and if n = 1, it acts as an ideal capacitor [57,58,59,60,61,62,63,64]. It is noticed that the Rpo and Rct significantly increase as the WCA increases. Increasing the WCA form 141° ± 2° to 147° ± 1° of the hydrophobic coatings has a significant influence on increasing the Rct from 102 kΩ·cm2 of PS1 to 140 kΩ·cm2 of PS3. However, increasing the WCA to 151° ± 2.8° and 155° ± 1.9° and decreasing the CAH to 7 ± 2.3 and 3 ± 4.2 leads to a remarkable increase of the Rct to three orders of magnitude (8 and 18 × 106 kΩ·cm2) in comparison to the uncoated Al, respectively. On the other hand, Cdl1 and Cdl2 of the SHCs distinctly is decreased to very low values in comparison to the uncoated and PS-coated Al substrates (PS1 and PS3), which indicates a low permeation of the electrolyte to the SHC/metal surface and a polarization resistance. It is worth mentioning that the shape of the phase angle of the uncoated and the coated Al (see Figure 8a,c), is not changed, which could be ascribed to the electrolyte permeation through the coating defects. The high corrosion resistance of the as prepared SHCs can be attributed to the trapped air in the disproportions of the heterogeneous surface, which prevents the aggressive ions from easily attacking the underlying surface of Al alloy. Moreover, the hydrophobic PS is non-polar and very good electrical insulator; therefore, aggressive ions can hardly transport through such coatings and reach the metal surface, thereby showing a superior corrosion resistance via physical modification of its surface.

4. Conclusions

The different electrospinning operational parameters have a great influence on the morphology, surface roughness, and wettability of the pure PS and PS/Al2O3 nanocomposite coatings. Also, the addition of Al2O3 nanoparticles markedly increases the surface roughness. The highest WCA is measured for the nanocomposite PA3 (which has the highest surface roughness with an Ra of 82 ± 2 nm) and was found to be 155° ± 1.9°. On the other hand, increasing the PS concentration is not recommended to increase the WCA. In addition, it is revealed that increasing the nanofiber diameter decreases the WCA and increases the CAH. The optimum conditions of electrospinning in order to obtain the highest possible water contact angle (155° ± 1.9°), and low sliding angle 3 ± 4.2, are a flow rate of 1.5 mL·h−1 and an applied voltage of 25 kV with polystyrene: an Al2O3 ratio of 1:10. In addition, the higher the WCA, the higher the corrosion resistance and the lower WCAH are. The combination of the micro-nano structure of the beaded fiber morphology results in high WCA and low WCAH. Despite their highly porous nature, the as-synthesized SHCs (PA1 & PA3) significantly increased the corrosion resistance of Al in saline water more than three orders of magnitude.

Acknowledgments

This publication was supported by Qatar University Internal Grant No. GCC-2017-012. The findings achieved herein are solely the responsibility of the authors. Thanks are also due to Anton Popelka for assistance with the AFM analysis.

Author Contributions

Ahmed Bahgat Radwan performed all the experiments and helped write some parts of the manuscript. Aboubakr M. Abdullah designed the whole corrosion work besides some of the superhydrophobic work, wrote parts of the manuscript, and reviewed it as a whole. Adel M. A. Mohamed designed most of the superhydrophobic work, was involved in all of the discussions, and helped write the manuscript. Mariam A. Al-Maadeed was responsible for the coating characterization.

Conflicts of Interest

The author declares no conflict of interest.

References

  1. Nakajima, A.; Fujishima, A.; Hashimoto, K.; Watanabe, T. Preparation of transparent superhydrophobic boehmite and silica films by sublimation of aluminum acetylacetonate. Adv. Mater. 1999, 11, 1365–1368. [Google Scholar] [CrossRef]
  2. Schindelholz, E.; Kelly Robert, G. Wetting phenomena and time of wetness in atmospheric corrosion: A review. Corros. Rev. 2012, 30, 135–170. [Google Scholar] [CrossRef]
  3. Bhushan, B.; Jung, Y.C.; Koch, K. Self-cleaning efficiency of artificial superhydrophobic surfaces. Langmuir 2009, 25, 3240–3248. [Google Scholar] [CrossRef] [PubMed]
  4. Sun, T.; Tan, H.; Han, D.; Fu, Q.; Jiang, L. No platelet can adhere—Largely improved blood compatibility on nanostructured superhydrophobic surfaces. Small 2005, 1, 959–963. [Google Scholar] [CrossRef] [PubMed]
  5. Ishizaki, T.; Saito, N. Rapid formation of a superhydrophobic surface on a magnesium alloy coated with a cerium oxide film by a simple immersion process at room temperature and its chemical stability. Langmuir 2010, 26, 9749–9755. [Google Scholar] [CrossRef] [PubMed]
  6. Jin, S.; Choi, C. Superhydrophobic and Superoleophobic Nano Surfaces Used as Antifingerprint Touch Sensitive Screen. WO Patent Application No. 2012087352A2, 28 June 2012. [Google Scholar]
  7. Zhang, L.; Wu, J.; Hedhili, M.N.; Yang, X.; Wang, P. Inkjet printing for direct micropatterning of a superhydrophobic surface: Toward biomimetic fog harvesting surfaces. J. Mater. Chem. A 2015, 3, 2844–2852. [Google Scholar] [CrossRef]
  8. Zhou, Z.; Fa, W.X. Electrospinning superhydrophobic-superoleophilic fibrous PVDF membranes for high-efficiency water-oil separation. Mater. Lett. 2015, 160, 423–427. [Google Scholar] [CrossRef]
  9. Lapierre, F.; Harnois, M.; Coffinier, Y.; Boukherroub, R.; Thomy, V. Split and flow: Reconfigurable capillary connection for digital microfluidic devices. Lab Chip 2014, 14, 3589–3593. [Google Scholar] [CrossRef] [PubMed]
  10. Ivanova, E.P.; Hasan, J.; Webb, H.K.; Truong, V.K.; Watson, G.S.; Watson, J.A.; Baulin, V.A.; Pogodin, S.; Wang, J.Y.; Tobin, M.J.; et al. Natural bactericidal surfaces: Mechanical rupture of pseudomonas aeruginosa cells by cicada wings. Small 2012, 8, 2489–2494. [Google Scholar] [CrossRef] [PubMed]
  11. Gao, X.; Jiang, L. Biophysics: Water-repellent legs of water striders. Nature 2004, 432, 36. [Google Scholar] [CrossRef] [PubMed]
  12. Hu, D.L.; Bush, J.W.M. Meniscus-climbing insects. Nature 2005, 437, 733–736. [Google Scholar] [CrossRef] [PubMed]
  13. Liu, K.; Du, J.; Wu, J.; Jiang, L. Superhydrophobic gecko feet with high adhesive forces towards water and their bio-inspired materials. Nanoscale 2012, 4, 768–772. [Google Scholar] [CrossRef] [PubMed]
  14. Min, W.L.; Jiang, B.; Jiang, P. Bioinspired self-cleaning antireflection coatings. Adv. Mater. 2008, 20, 3914–3918. [Google Scholar] [CrossRef]
  15. Bayer, I. On the durability and wear resistance of transparent superhydrophobic coatings. Coatings 2017, 7, 12. [Google Scholar] [CrossRef]
  16. Heib, F.; Schmitt, M. Statistical contact angle analyses with the high-precision drop shape analysis (HPDSA) approach: Basic principles and applications. Coatings 2016, 6, 57. [Google Scholar] [CrossRef]
  17. Lee, K.-M.; Ngo, C.V.; Jeong, J.Y.; Jeon, E.-C.; Je, T.J.; Chun, D.M. Fabrication of an anisotropic superhydrophobic polymer surface using compression molding and dip coating. Coatings 2017, 7, 194. [Google Scholar] [CrossRef]
  18. Fontananova, E.; Jansen, J.C.; Cristiano, A.; Curcio, E.; Drioli, E. Effect of additives in the casting solution on the formation of pvdf membranes. Desalination 2006, 192, 190–197. [Google Scholar] [CrossRef]
  19. Anton, F. Process and Apparatus for Preparing Artificial Threads. U.S. Patent Application No. 1975504A, 2 October 1934. [Google Scholar]
  20. Huang, Z.M.; Zhang, Y.Z.; Kotaki, M.; Ramakrishna, S. A review on polymer nanofibers by electrospinning and their applications in nanocomposites. Compos. Sci. Technol. 2003, 63, 2223–2253. [Google Scholar] [CrossRef]
  21. Deitzel, J.M.; Kleinmeyer, J.; Harris, D.; Beck Tan, N.C. The effect of processing variables on the morphology of electrospun nanofibers and textiles. Polymer 2001, 42, 261–272. [Google Scholar] [CrossRef]
  22. Sukigara, S.; Gandhi, M.; Ayutsede, J.; Micklus, M.; Ko, F. Regeneration of bombyx mori silk by electrospinning—Part 1: Processing parameters and geometric properties. Polymer 2003, 44, 5721–5727. [Google Scholar] [CrossRef]
  23. Demir, M.M.; Yilgor, I.; Yilgor, E.; Erman, B. Electrospinning of polyurethane fibers. Polymer 2002, 43, 3303–3309. [Google Scholar] [CrossRef]
  24. Fong, H.; Chun, I.; Reneker, D.H. Beaded nanofibers formed during electrospinning. Polymer 1999, 40, 4585–4592. [Google Scholar] [CrossRef]
  25. Ondarçuhu, T.; Joachim, C. Drawing a single nanofibre over hundreds of microns. Europhys. Lett. 1998, 42, 215. [Google Scholar] [CrossRef]
  26. Feng, L.; Li, S.; Li, H.; Zhai, J.; Song, Y.; Jiang, L.; Zhu, D. Super-hydrophobic surface of aligned polyacrylonitrile nanofibers. Angew. Chem. Int. Ed. 2002, 41, 1221–1223. [Google Scholar] [CrossRef]
  27. Ma, P.X.; Zhang, R. Synthetic nano-scale fibrous extracellular matrix. J. Biomed. Mater. Res. 1999, 46, 60–72. [Google Scholar] [CrossRef]
  28. Liu, G.; Qiao, L.; Guo, A. Diblock copolymer nanofibers. Macromolecules 1996, 29, 5508–5510. [Google Scholar] [CrossRef]
  29. Doshi, J.; Reneker, D.H. Electrospinning process and applications of electrospun fibers. J. Electrostat. 1995, 35, 151–160. [Google Scholar] [CrossRef]
  30. Mohamed, M.A.; Abdullah, A.B.; Al-Maadeed, M.; Radwan, A.B. Fundamental, fabrication and applications of superhydrophobic surfaces fabrication and applications of superhydrophobic surfaces. In Research Perspectives on Functional Micro-and Nanoscale Coatings; Zuzuarregui, A., Morant-Miñana, M.C., Eds.; IGI Global: Hershey, PA, USA, 2016; pp. 341–368. [Google Scholar]
  31. Radwan, A.B.; Abdullah, A.B.; Alnuaimi, N.A. Recent advances in corrosion resistant superhydrophobic coatings. Corros. Rev. 2017. [Google Scholar] [CrossRef]
  32. Lee, K.H.; Kim, H.Y.; Bang, H.J.; Jung, Y.H.; Lee, S.G. The change of bead morphology formed on electrospun polystyrene fibers. Polymer 2003, 44, 4029–4034. [Google Scholar] [CrossRef]
  33. Maul, J.; Frushour, B.G.; Kontoff, J.R.; Eichenauer, H.; Ott, K.H.; Schade, C. Polystyrene and styrene copolymers. In Ullmann's Encyclopedia of Industrial Chemistry; Wiley-VCH Verlag GmbH & Co. KGaA: Weinheim, Germany, 2000. [Google Scholar]
  34. Jarusuwannapoom, T.; Hongrojjanawiwat, W.; Jitjaicham, S.; Wannatong, L.; Nithitanakul, M.; Pattamaprom, C.; Koombhongse, P.; Rangkupan, R.; Supaphol, P. Effect of solvents on electro-spinnability of polystyrene solutions and morphological appearance of resulting electrospun polystyrene fibers. Eur. Polym. J. 2005, 41, 409–421. [Google Scholar] [CrossRef]
  35. Acatay, K.; Simsek, E.; Ow-Yang, C.; Menceloglu, Y.Z. Tunable, superhydrophobically stable polymeric surfaces by electrospinning. Angew. Chem. Int. Ed. 2004, 116, 5322–5325. [Google Scholar] [CrossRef]
  36. Hou, W.; Wang, Q. Wetting behavior of a SiO2-polystyrene nanocomposite surface. J. Colloid Interface Sci. 2007, 316, 206–209. [Google Scholar] [CrossRef] [PubMed]
  37. Hou, W.; Wang, Q. UV-driven reversible switching of a polystyrene/titania nanocomposite coating between superhydrophobicity and superhydrophilicity. Langmuir 2009, 25, 6875–6879. [Google Scholar] [CrossRef] [PubMed]
  38. Xu, X.; Zhang, Z.; Guo, F.; Yang, J.; Zhu, X.; Zhou, X.; Xue, Q. Fabrication of bionic superhydrophobic manganese oxide/polystyrene nanocomposite coating. J. Bionic Eng. 2012, 9, 11–17. [Google Scholar] [CrossRef]
  39. Wang, Y.; Li, B.; Liu, T.; Xu, C.; Ge, Z. Controllable fabrication of superhydrophobic TiO2 coating with improved transparency and thermostability. Colloids Surf. A 2014, 441, 298–305. [Google Scholar] [CrossRef]
  40. Hart, L.D. Alumina Chemicals: Science and Technology Handbook; American Ceramic Society: Columbus, OH, USA, 1990. [Google Scholar]
  41. Keyvani, A.; Saremi, M.; Heydarzadeh Sohi, M. Microstructural stability of zirconia–alumina composite coatings during hot corrosion test at 1050 °C. J. Alloys Compd. 2010, 506, 103–108. [Google Scholar] [CrossRef]
  42. Zhan, N.; Li, Y.; Zhang, C.; Song, Y.; Wang, H.; Sun, L.; Yang, Q.; Hong, X. A novel multinozzle electrospinning process for preparing superhydrophobic PS films with controllable bead-on-string/microfiber morphology. J. Colloid Interface Sci. 2010, 345, 491–495. [Google Scholar] [CrossRef] [PubMed]
  43. Lee, J.S.; Choi, K.H.; Ghim, H.D.; Kim, S.S.; Chun, D.H.; Kim, H.Y.; Lyoo, W.S. Role of molecular weight of atactic poly(vinyl alcohol) (PVA) in the structure and properties of PVA nanofabric prepared by electrospinning. J. Appl. Polym. Sci. 2004, 93, 1638–1646. [Google Scholar] [CrossRef]
  44. Megelski, S.; Stephens, J.S.; Chase, D.B.; Rabolt, J.F. Micro- and nanostructured surface morphology on electrospun polymer fibers. Macromolecules 2002, 35, 8456–8466. [Google Scholar] [CrossRef]
  45. Baumgarten, P.K. Electrostatic spinning of acrylic microfibers. J. Colloid Interface Sci. 1971, 36, 71–79. [Google Scholar] [CrossRef]
  46. Kim, E.S.; Kim, S.H.; Lee, C.H. Electrospinning of polylactide fibers containing silver nanoparticles. Macromol. Res. 2010, 45, 215–221. [Google Scholar] [CrossRef]
  47. Tuberquia, J.C.; Nizamidin, N.; Robert, R.; Harl, R.R.; Albert, J.; Hunter, J.; Rogers, B.R.; Kane, G.J. Surface-Initiated Polymerization of Superhydrophobic Polymethylene. J. Am. Chem. Soc. 2010, 132, 5725–5734. [Google Scholar] [CrossRef] [PubMed]
  48. Wenzel, R.N. Resistance of solid surfaces to wetting by water. Ind. Eng. Chem. 1936, 28, 988–994. [Google Scholar] [CrossRef]
  49. Cassie, A.B.D.; Baxter, S. Wettability of porous surfaces. Trans. Faraday Soc. 1944, 40, 546–551. [Google Scholar] [CrossRef]
  50. Quere, D. Surface chemistry: Fakir droplets. Nat. Mater. 2002, 1, 14–15. [Google Scholar] [CrossRef] [PubMed]
  51. Conti, J.; De Coninck, J.; Ghazzal, M.N. Design of water-repellant coating using dual scale size of hybrid silica nanoparticles on polymer surface. Appl. Surf. Sci. 2018, 436, 234–241. [Google Scholar] [CrossRef]
  52. Karapanagiotis, I.; Manoudis, P.N.; Savva, A.; Panayiotou, C. Superhydrophobic polymer-particle composite films produced using various particle sizes. Surf. Interface Anal. 2012, 44, 870–875. [Google Scholar] [CrossRef]
  53. Manoudis, P.N.; Karapanagiotis, I. Modification of the wettability of polymer surfaces using nanoparticles. Prog. Org. Coat. 2014, 77, 331–338. [Google Scholar] [CrossRef]
  54. Wang, Y.; Suryanarayana, C.; An, L. Phase transformation in nanometer-sized γ-alumina by mechanical milling. J. Am. Ceram. Soc. 2005, 88, 780–783. [Google Scholar] [CrossRef]
  55. Ghezelbash, Z.; Ashouri, D.; Mousavian, S.; Ghandi, A.H.; Rahnama, Y. Surface modified Al2O3 in fluorinated polyimide/Al2O3 nanocomposites: Synthesis and characterization. Bull. Mater. Sci. 2012, 35, 925–931. [Google Scholar] [CrossRef]
  56. Radwan, A.B.; Mohamed, A.M.A.; Abdullah, A.M.; Al-Maadeed, M.A. Corrosion protection of electrospun pvdf–ZnO superhydrophobic coating. Surf. Coat. Technol. 2016, 289, 136–143. [Google Scholar] [CrossRef]
  57. Tang, C.; Stueber, M.; Seifert Hans, J.; Steinbrueck, M. Protective coatings on zirconium-based alloys as accident-tolerant fuel (ATF) claddings. Corros. Rev. 2017, 35, 141–165. [Google Scholar] [CrossRef]
  58. Kadapparambil, S.; Yadav, K.; Ramachandran, M.; Victoria Selvam, N. Electrochemical investigation of the corrosion inhibition mechanism of tectona grandis leaf extract for SS304 stainless steel in hydrochloric acid. Corros. Rev. 2017, 35, 111–121. [Google Scholar] [CrossRef]
  59. Kumar, R.; Chahal, S.; Dahiya, S.; Dahiya, N.; Kumar, S.; Lata, S. Experimental and theoretical approach to exploit the corrosion inhibition activity of 3-formyl chromone derivatives on mild steel in 1 M H2SO4. Corros. Rev. 2017, 35, 95–110. [Google Scholar] [CrossRef]
  60. Dahiya, S.; Lata, S.; Kumar, P.; Kumar, R. A descriptive study for corrosion control of low-alloy steel by aloe vera extract in acidic medium. Corros. Rev. 2016, 34, 241–248. [Google Scholar] [CrossRef]
  61. Fayyad, E.; Abdullah, A.; Hassan, M.; Mohamed, A.; Wang, C.; Jarjoura, G.; Farhat, Z. Synthesis, characterization, and application of novel Ni-P-carbon nitride nanocomposites. Coatings 2018, 8, 37. [Google Scholar] [CrossRef]
  62. Bai, Y.; Xing, J.; Guo, Y.; Li, J.; Huang, Q.; Gao, Y. Influence of 4 wt % Cr addition on the corrosion-wear synergistic effect for Al2O3/Fe(Al) composites. Corros. Rev. 2016, 34, 231–240. [Google Scholar] [CrossRef]
  63. Książek, M. Resistance to chemical attack of cement composites impregnated with a special polymer sulfur composite. Corros. Rev. 2016, 34, 211–229. [Google Scholar] [CrossRef]
  64. Yang, D.; Liu, S.H.; Shao, Y.P.; Di Xu, S.; Zhao, L.L.; Liao, Q.Q.; Ge, H.H. Electrochemical and XPS studies of alkyl imidazoline on the corrosion inhibition of carbon steel in citric acid solution. Corros. Rev. 2016, 34, 295–304. [Google Scholar] [CrossRef]
Figure 1. SEM micrographs of the as prepared PS coating without any addition of Al2O3 nanoparticles for (a) PS1, (b) PS2, (c) PS3, and (d) PS4 (See Table 1 for the operational parameters).
Figure 1. SEM micrographs of the as prepared PS coating without any addition of Al2O3 nanoparticles for (a) PS1, (b) PS2, (c) PS3, and (d) PS4 (See Table 1 for the operational parameters).
Coatings 08 00065 g001
Figure 2. The SEM images of PS/Al2O3 nanocomposite coating for (a) PA1, (b) PA2, (c) PA3, and (d) PA4 (See Table 1 for Operational parameters).
Figure 2. The SEM images of PS/Al2O3 nanocomposite coating for (a) PA1, (b) PA2, (c) PA3, and (d) PA4 (See Table 1 for Operational parameters).
Coatings 08 00065 g002aCoatings 08 00065 g002b
Figure 3. The SEM/EDX mapping micrographs of the as-prepared SHCS (a) PA1 and (b) PA3.
Figure 3. The SEM/EDX mapping micrographs of the as-prepared SHCS (a) PA1 and (b) PA3.
Coatings 08 00065 g003
Figure 4. Snapshots of the measured water contact angle after and before the addition of Al2O3 nanoparticles.
Figure 4. Snapshots of the measured water contact angle after and before the addition of Al2O3 nanoparticles.
Coatings 08 00065 g004
Figure 5. FTIR for (a) Al2O3 nanoparticles, (b) PS1, (c) PS2, (d) PS3, (e) PS4, (f) PA1, (g) PA2, (h) PA3, and (i) PA4.
Figure 5. FTIR for (a) Al2O3 nanoparticles, (b) PS1, (c) PS2, (d) PS3, (e) PS4, (f) PA1, (g) PA2, (h) PA3, and (i) PA4.
Coatings 08 00065 g005
Figure 6. AFM 3D images for (a) PS1, (b) PS2, (c) PS3, (d) PS4, (e) PA1, (f) PA2, (g) PA3, and (h) PA4.
Figure 6. AFM 3D images for (a) PS1, (b) PS2, (c) PS3, (d) PS4, (e) PA1, (f) PA2, (g) PA3, and (h) PA4.
Coatings 08 00065 g006
Figure 7. Nyquist plots of the (a) uncoated Al alloy (b) PS1, (c) PS3, (d) PA1, and (e) PA3 from the EIS measurements in 3.5 wt % NaCl.
Figure 7. Nyquist plots of the (a) uncoated Al alloy (b) PS1, (c) PS3, (d) PA1, and (e) PA3 from the EIS measurements in 3.5 wt % NaCl.
Coatings 08 00065 g007
Figure 8. Bode plots of the (a) uncoated Al alloy (b) PS1, (c) PS3, (d) PA1, and (e) PA3 from the EIS measurements in 3.5 wt % NaCl.
Figure 8. Bode plots of the (a) uncoated Al alloy (b) PS1, (c) PS3, (d) PA1, and (e) PA3 from the EIS measurements in 3.5 wt % NaCl.
Coatings 08 00065 g008aCoatings 08 00065 g008b
Figure 9. Equivalent electrical circuit used to fit the EIS spectra of the uncoated Al alloy and the as-prepared SHCs in saline water.
Figure 9. Equivalent electrical circuit used to fit the EIS spectra of the uncoated Al alloy and the as-prepared SHCs in saline water.
Coatings 08 00065 g009
Table 1. Compositional ratios and electrospinning operational parameters for pure PS and PS/Al2O3 nanocomposite coatings.
Table 1. Compositional ratios and electrospinning operational parameters for pure PS and PS/Al2O3 nanocomposite coatings.
Exp. CodePS (wt %)Al2O3 (wt %)Potential (kV)Flow Rate (mL·h−1)
PS12.5201.5
PS22.5252
PS32.5251.5
PS45251.5
PA12.50.25201.5
PA22.50.35252
PA32.50.25251.5
PA450.25251.5
Table 2. The average diameter of the nanofibers and beads of PS and PS/Al2O3 nanocomposite coatings.
Table 2. The average diameter of the nanofibers and beads of PS and PS/Al2O3 nanocomposite coatings.
PS CodesAverage Fiber Diameter (nm)PA Codes (PS/Al2O3)Average Fiber Diameter (nm)
PS1340 ±27PA1325 ±23
PS2328 ±29PA2315 ±27
PS3320 ±21PA3290 ±34
PS4433 ±15PA4413 ±21
Table 3. WCA and CAH of the prepared PS and PS/Al2O3 nanocomposite coatings.
Table 3. WCA and CAH of the prepared PS and PS/Al2O3 nanocomposite coatings.
CodeWCAWCAH
PS1141° ± 2°24° ± 3°
PS2143° ± 3°20° ± 4°
PS3147° ± 1°14° ± 3°
PS4138° ± 2°32° ± 6°
PA1151° ± 2.8°7° ± 2.3°
PA2152° ± 1.2°5° ± 3.1°
PA3155° ± 1.9°3° ± 4.2°
PA4147° ± 2°13° ± 3°
Table 4. The Ra values of PS and PS/Al2O3 nanocomposite coatings.
Table 4. The Ra values of PS and PS/Al2O3 nanocomposite coatings.
CodesRa Values (nm)
PS122 ± 2
PS226 ± 4
PS332 ± 3
PS417 ± 4
PA153 ± 3
PA261 ± 4
PA382 ± 2
PA427 ± 3
Table 5. The electrochemical parameters from Nyquist and Bode plots for the uncoated and coated aluminum substrates with pure electrospun PS (PS1 & PS3), and nanocomposite SHCs of polystyrene and aluminum oxide (PA1 & PA3), in 3.5 wt % NaCl solution.
Table 5. The electrochemical parameters from Nyquist and Bode plots for the uncoated and coated aluminum substrates with pure electrospun PS (PS1 & PS3), and nanocomposite SHCs of polystyrene and aluminum oxide (PA1 & PA3), in 3.5 wt % NaCl solution.
SamplesWCA
(°)
Rpo
(kΩ·cm2)
Rct
(kΩ·cm2)
Y01
−1·cm−2·sn) × 10−6
n1Cdl1
(μF·cm−2)
Y02
−1·cm−2·sn) × 10−6
n2Cdl2
(μF·cm−2)
uncoated Al alloy87 ± 20.7411000.83315001480.763120
PS1141 ± 277102280.7354140.7012.7
PS3147 ± 122014080.7148.31.80.6970.98
PA1151 ± 2.853080000.0480.6920.0330.0040.4083.4 × 10−5
PA3155 ± 1.9860180000.0130.5850.00470.00120.2632.5 × 10−8

Share and Cite

MDPI and ACS Style

Bahgat Radwan, A.; Abdullah, A.M.; Mohamed, A.M.A.; Al-Maadeed, M.A. New Electrospun Polystyrene/Al2O3 Nanocomposite Superhydrophobic Coatings; Synthesis, Characterization, and Application. Coatings 2018, 8, 65. https://doi.org/10.3390/coatings8020065

AMA Style

Bahgat Radwan A, Abdullah AM, Mohamed AMA, Al-Maadeed MA. New Electrospun Polystyrene/Al2O3 Nanocomposite Superhydrophobic Coatings; Synthesis, Characterization, and Application. Coatings. 2018; 8(2):65. https://doi.org/10.3390/coatings8020065

Chicago/Turabian Style

Bahgat Radwan, Ahmed, Aboubakr M. Abdullah, Adel M. A. Mohamed, and Mariam A. Al-Maadeed. 2018. "New Electrospun Polystyrene/Al2O3 Nanocomposite Superhydrophobic Coatings; Synthesis, Characterization, and Application" Coatings 8, no. 2: 65. https://doi.org/10.3390/coatings8020065

APA Style

Bahgat Radwan, A., Abdullah, A. M., Mohamed, A. M. A., & Al-Maadeed, M. A. (2018). New Electrospun Polystyrene/Al2O3 Nanocomposite Superhydrophobic Coatings; Synthesis, Characterization, and Application. Coatings, 8(2), 65. https://doi.org/10.3390/coatings8020065

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop