1. Introduction
Cubic boron nitride (c-BN), an analog of diamond, exhibits many outstanding properties, such as extreme hardness, wide band gap, negative electron affinity, and high thermal conductivity. Furthermore, c-BN also has numerous properties, such as higher chemical stability, both p- and n-type doping availability, surface smoothness, biocompatibility, and hydrophilicity, that make it superior to diamond for applications in protection coatings and cutting tools, high-temperature electronics, ultraviolet (UV) detectors, deep-UV light-emitting diodes, and bio-/chemi-sensors [
1,
2]. However, synthesizing device-quality large-area single crystals of c-BN has not been established despite considerable progress [
3,
4,
5] and single crystal wafers are not available yet.
So far, various techniques have been employed to grow c-BN films, including physical vapor deposition [
3,
6] and plasma-enhanced chemical vapor deposition [
7,
8]. The energetic plasma surface process is essential for the nucleation and growth of c-BN thin films regardless of growth technique. The chemical routes usually use deleterious and corrosive gases, such as H, C, Na, F, Ar, and He, unavoidably leaving contaminants in c-BN films. The uncontrolled presence of impurities involved in the growth process leads to uncertainty of the electronic transport mechanism in intrinsic samples, which is mirrored by the fact that numerous luminescence centers have been observed in c-BN crystals prepared by high-pressure, high-temperature synthesis, and for many of those it is not clear whether they can be attributed to an intrinsic defect or to a precursor impurity [
9,
10,
11,
12]. On the other hand, most physical vapor deposition methods rely on either energetic ion bombardment with the substrate being negatively biased or electron assistance with the substrate being positively biased, which is generally assisted by massive ions of Ar [
13,
14]. Such involvement of Ar ions may cause resputter of the deposited film, structural damage, and stress accumulation, especially under high ion energy conditions [
15,
16]. Although introducing H
2 into the working gases can effectively etch the
sp2 phase, leaving an
sp3 phase [
17], the assistance of Ar for energetic ion bombardment is the major reason for the poor adhesion that is usually found, which severely hinders the application of c-BN films.
Hofsass et al. [
18] attempted to grow c-BN film by using only 11B
+ and 14N
+ ions on heated Si substrates in ultra-high vacuum (UHV) environment using mass separated ion beam deposition. For the first time, no additional ions, such as Ar
+, were involved in the growth process. Litvinov et al. [
19] obtained thick c-BN films with reduced bias voltage in pure nitrogen gas using an electron cyclotron resonance source. Later, Yap et al. [
20] investigated c-BN films using plasma-assisted pulsed-laser deposition in pure N
2 radio frequency (RF) plasma. They found that all c-BN films prepared in pure N
2 plasma were significantly improved in stability versus those prepared in Ar-rich plasma. These approaches, however, normally require a complex apparatus and are energy consuming. Thus, it is critical to find a simple and effective way to synthesize high-quality c-BN films by using growth species such as B
+ and N
+ ions exclusively.
Diamond has been reported as a perfect nucleation surface for epitaxial growth of c-BN due to the small lattice mismatch of these two materials [
3,
4,
21,
22]. Epitaxy of c-BN/diamond is attracting significant attention for both basic crystal engineering and optoelectronic applications. From this point of view, imitating nucleation of c-BN on diamond surface is very interesting, as well as the growth of high-quality c-BN films. As has been demonstrated previously [
23], the deposition of a thin h-BN interfacial layer followed by an intended c-BN film can provide a pure c-BN polycrystalline top layer as a nucleation template for subsequent growth. Generally, elevated substrate temperatures combined with significantly enhanced ion bombardment are needed in order to obtain the pure cubic phase at the growth layer. Here, we report on the deposition of high-quality c-BN films on Si substrates by the conventional RF magnetron sputter method without additional argon ion bombardment. An important aspect previously overlooked in the deposition process of c-BN film is optimization of the experimental parameters using pure N
2 gas in nucleation and growth. We therefore focus on characterization of the c-BN films prepared using pure N
2 or mixed Ar/N
2 plasma with different deposition times, which enables investigation of the difference between these two parameters in the initial nucleation stage of the films. The pure-phase c-BN growth window is obtained when using pure N
2 gas. Furthermore, using pure N
2 gas instead of additional Ar results in improved microstructure quality and much reduced compressive stress, suggesting a fundamental strategy for achieving high-quality c-BN films.
3. Results and Discussion
Figure 1a shows the FTIR spectra obtained from BN films using pure N
2 plasma at 470 °C with different deposition times. The absorption band at 1091 cm
−1 is due to the transverse optical (TO) mode of c-BN, while two absorption bands at 1400 and 770 cm
−1 correspond to the h-BN phase and result from the in-plane B–N stretching mode and the out-of-plane B–N–B bending vibration, respectively [
17]. It can be clearly observed that there is a continuous increase of the intensity of c-BN peak, while the positions of the c-BN peaks have no obvious shift with increased deposition time. The intensity of the h-BN absorption peaks exhibits no obvious change. The IR absorption spectra of BN films using 1:1 Ar/N
2 plasma at different deposition times are displayed in
Figure 1b. In this case, the absorption bands of all c-BN films stay at 1100 cm
−1. With increased deposition time, the intensity of c-BN peak also increases, whereas no obvious shift is observed for its position. Compared to the film grown using pure N
2, it is noticeable that at the deposition time of 10 min, the film grown using Ar/N
2 already exhibits trivial cubic phases, which suggests that involvement of Ar during the film deposition causes the cubic phase to nucleate faster than the one using pure N
2. The cubic volume fraction can be estimated directly from relative intensities of the c-BN TO peak (
Ic-BN) and the h-BN peak at 1400 cm
−1 (
Ih-BN):
Thus, we can estimate the cubic volume fraction of each film, which is 47%, 60%, and 70% for the film using pure N2 and 50%, 71%, and 80% for the film using Ar/N2. The cubic phase content in the c-BN films using Ar/N2 plasma is higher than that using pure N2 plasma at the same deposition time, since the increased bombardment of the c-BN films by energetic Ar ions induces a higher growth rate. The thickness of the film prepared using Ar/N2 for 40 min is about 50 nm, corresponding to a growth rate of 1.25 nm/min, while the growth rate of the film prepared using pure N2 is slightly lower (~1.12 nm/min).
In addition, the positions of c-BN TO mode peaks shift toward the lower wavenumber direction for the films grown in pure N
2 plasma compared to those using mixed Ar/N
2 plasma. The compressive stress for the film can be estimated from
This strongly indicates reduced compressive stress in the c-BN film without additional argon ion bombardment [
24]. Both c-BN films grown, regardless of additional Ar ion bombardment, reveal the well-known layered structure of amorphous/hexagonal/cubic phases, which are confirmed by the following surface characterizations. The thickness of the initial layer of hexagonal structure estimated from the
sp2 absorbance and an absorbance coefficient (h-BN: 25,000 cm
−1) was approximately 15 nm for the film grown using pure N
2 plasma and 10 nm for the film grown using Ar/N
2 plasma [
25]. It has also been observed that an increase in the N
2 plasma concentration extends the thickness of the interlayer [
26].
It is well known that fluctuations in the near surface atomic structure of the studied films will lead to variations in the density and, consequently, the plasmon energies. Energy loss function delivers more information on the influence of the near surface structure.
Figure 2a,b shows energy loss spectra based on N1s core level electron excitations of the BN films using pure N
2 plasma and Ar/N
2 plasma with different deposition times. For the films grown with deposition time from 10 to 40 min, minor variations are detected from the bottom to the top curve as far as the plasmon energy and the general shape of the loss function are concerned. A prominent peak can be observed at 8 eV in films grown using either pure N
2 or Ar/N
2 with a deposition time of 10 min. In the BN system, the peak at 8 eV is due to a π–π* interband transition [
27], which can only occur in h-BN, thus acts as a fingerprint for h-BN. The peak located at about 27 eV is attributed to the volume plasmon of h-BN as well. This indicates that the surface of the films is composed mainly of the h-BN phase at the initial nucleation stage. With longer deposition time, differences in the h-BN and c-BN loss functions are visible as increased plasmon energy in the cubic phase reflecting the higher density, accompanied by the absence of π–π* related features, attenuation of the volume plasmon of h-BN, and the appearance of additional structures at energies higher than 30 eV [
28,
29]. These results unambiguously reflect the layered structure of amorphous/hexagonal/cubic phases. Another important detail of the loss spectrum for the BN film grown using pure N
2 gas for 10 min is that the small peak at about 4.6 eV is due to the N–N bonds [
30], which is invisible for the film grown using Ar/N
2. This strongly suggests the existence of N–N configurations in hexagonal BN layer supplied by pure N
2 bombardment at the initial stage.
To gain further insight into the differences in the nucleation process of c-BN films using pure N
2 plasma and mixed Ar/N
2 plasma, a nucleation sequence was studied in detail by means of AFM measurements.
Figure 3 presents root mean squared (RMS) roughness as a function of deposition time. Typical AFM images recorded as surface morphology for these films are shown in
Figure S5. Several AFM images were taken at different positions for each film surface for the RMS estimation. Thus it was expected that the errors involved were random and could be cancelled out when statistical results were averaged. After 10 min of growth, the RMS roughness of the films was estimated as 0.74 ± 0.04 nm and 1.20 ± 0.07 nm for pure N
2 plasma and mixed Ar/N
2 plasma, respectively. It is known from FTIR measurements and energy loss functions that the film for pure N
2 growth consists mainly of h-BN after 10 min; however, the cubic phase already starts to nucleate for the film grown with Ar/N
2. It was previously reported that bombardment of Ar ions can penetrate into the growing h-BN film during deposition and induce accumulation of compressive stress, consequently influencing the microstructure of the h-BN layer [
31]. As a result, the initial h-BN layer becomes rougher, since a randomly oriented laminate structure forms under the ion bombardment. Such bombardment leads to high enough compressive stresses to favor c-BN thermodynamically. It is believed that the higher roughness of h-BN film grown with argon ion bombardment is caused by Ar
+ ion penetration into the film during deposition. In order to confirm this speculation, the XPS spectra of survey and Ar 2
p core level (
Figure 4) for the BN films deposited for 10 min were measured. This clearly shows that the Ar ions reside in the BN film prepared in Ar/N
2 plasma. However, there is no contaminant of Ar in h-BN film grown without Ar ion bombardment. It has been reported that residual stress of h-BN is reduced after annealing at high temperature, which also explains how the buried Ar atoms could diffuse out during annealing [
24].
As the deposition time increases more than 10 min and the subsequent cubic structure accumulates continuously, the surface of the c-BN films prepared in Ar/N
2 plasma becomes very smooth. The RMS roughness of these films with deposition times of 20, 30, and 40 min was 0.81 ± 0.06 nm, 0.68 ± 0.04 nm, and 0.79 ± 0.05 nm, respectively. Contrarily, the RMS roughness of the pure N
2 prepared films with deposition times of 20, 30, and 40 min was estimated as 2.23 ± 0.10 nm, 2.75 ± 0.11 nm, and 1.26 ± 0.11 nm, respectively. Thus, the films prepared without argon ion bombardment were much rougher. After 40 min, the surface became smooth again. This was probably due to the fine crystallites of c-BN films with mixed Ar/N
2 plasma, considering higher energetic ion bombardment with the assistance of Ar during film growth. Furthermore, Ar ion bombardment has been found to prevent the growth of larger crystallites [
32]. Therefore, the film surface obtained was composed of fine crystallites of several to tens of nanometers in size. Nevertheless, both systems of the c-BN films showed rather smooth surface over a large area regardless of Ar (see
Supplementary Materials). The results of roughness estimation indicate that moderate ion bombardment without the use of Ar ions is expected to improve the crystalline quality.
To further study the differences in growth conditions using pure N
2 and Ar/N
2 plasma, we focused on the c-BN layers grown on c-BN template nucleate layer in a two-step manner, in which the top layer of c-BN was expected to provide pure growth information. In the first step, template c-BN films were prepared in pure N
2 plasma under −250 V substrate bias voltage at 470 °C for 30 min. The template c-BN film has been characterized as shown in the
Supplementary Materials. In the second step, the substrate temperature was increased up to 800 °C and depositions were performed for 40 min at substrate bias voltages of −125, −150, −200, −250, and −275 V.
Figure 5a,b show a series of FTIR absorption spectra of the second BN films at different bias voltages with pure N
2 plasma and Ar/N. The relative height of IR peak is related to the thickness of the film under investigation. For the bias voltage in this range, further growth of the film was observed. The thickness of the film grown at −150 V for both gas compositions was roughly measured to be 50 nm by Taly step. It can be observed that the growth rate at −150 V was higher than that at the other bias voltages. When the bias voltage was changed from −150 to −275 V, the etching rate was enhanced as well, resulting in a monotonously reduced growth rate. No further growth of films occurred after the second growth when the bias voltage was beyond −300 V, implying that the resputtering regime was reached.
In addition, the critical bias voltage was explored and compared when using pure N2 and Ar/N2 plasma. This critical value is considered to be necessary for incubation of c-BN nucleation. For the films at bias voltages of −150, −200, −250, and −275 V, it is clear that the FTIR spectra are dominated by only one peak, which is characteristic for the TO mode of the cubic phase. The absence of characteristic h-BN peaks strongly indicates 100% cubic phase without any h-BN. On the other hand, the cubic content of c-BN film at bias voltage of −125 V with Ar/N2 plasma was estimated to be 87%, significantly higher than that with pure N2 (30% of cubic phase after second growth). This shows the critical bias voltage for growth of the pure cubic phase of BN films and the dependence of the critical voltage on the working gas. Deposition of pure c-BN films using Ar/N2 was obtained at lower bias voltage than when using pure N2 gas in the present experiments. Nevertheless, in both cases, the pure cubic phase of BN films was obtained within the bias voltage window from −150 to −275 V.
Besides, one may notice that for both cases, c-BN TO peaks in the FTIR spectra shift toward lower frequencies with reduced bias voltage during growth. This shift is consistent with the reduced compressive stress in the films grown at lower bias [
33]. In order to better compare the differences, the c-BN TO peak positions of the pure cubic phase films at bias voltages of −150, −200, −250, and −275 V displayed in
Figure 5 were plotted as a function of substrate bias voltage in
Figure 6. For both working gas systems, the c-BN TO peak slightly shifts toward higher frequencies at the bias voltage of −250 V and further shifts toward lower frequencies gradually. Since only phase-pure cubic BN films were compared in the present case, the subsequent shifting of the c-BN peak position as bias voltage decreased is predominantly residual compressive stress due to ion bombardment because of their comparative film thickness. Another important aspect is that the c-BN TO peak frequencies of the films grown using pure N
2 ion bombardment were rather low compared with those of c-BN films grown using Ar/N
2 plasma at the same bias voltage, indicating lower residual compressive stress. This was confirmed by the observation that the high cubic content containing BN films using Ar as reactive gas often delaminated in air, whereas those using pure N
2 gas were much more stable after several months in air. This suggests that the moderate ion bombardment using pure N
2 gas is propitious to grow less stressed c-BN films, favoring the growth of highly stable and robust pure c-BN films.