A Novel Zero-Thermal-Quenching Red Phosphor with High Quantum Efficiency and Color Purity

College of Material Science and Engineering, Sichuan University, Chengdu 610065, China
*
Author to whom correspondence should be addressed.
Inorganics 2023, 11(10), 406; https://doi.org/10.3390/inorganics11100406
Submission received: 14 September 2023 / Revised: 5 October 2023 / Accepted: 12 October 2023 / Published: 15 October 2023

Abstract

:
In this paper, a series of K5La1-x(MoO4)4: xSm3+ and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Ln3+ (Ln = Sc, Y or Gd) red phosphors were prepared by calcining the mixed raw powders at 600 °C. Meanwhile, the composition and fluorescence properties of the phosphors, especially for the thermal stability, were analyzed in detail. The results indicate that the K5La1-x(MoO4)4: xSm3+ phosphors can be effectively excited at 401 nm and emit red light with three main peaks at 561 nm, 600 nm and 646 nm, attributed to the 4G5/26Hj/2 (j = 5, 7 and 9) energy transitions of the Sm3+ ion respectively, among which the K5La0.93(MoO4)4: 0.07Sm3+ exhibits the highest intensity. The quenching mechanism is ascribed to the dipole-dipole interaction. Ln3+ co-doping does not change the shape and peaking position of the excitation and emission spectra of K5La0.93(MoO4)4: 0.07Sm3+, but further increases the emission intensity in different degrees. Particularly, K5La0.86(MoO4)4: 0.07Sm3+, 0.07Gd3+ demonstrates a high quantum efficiency of 74.63%, a low color temperature (1753 K), and a high color purity of up to 99.97%. It is worth noting that all the phosphors have a good thermal stability, even a zero quenching phenomenon occurs, attributed to the electron traps confirmed by the TL spectrum.

1. Introduction

Compared with traditional lighting methods, the new generation of LED lighting has a relatively longer life expectancy, produces less heat and consumes less energy with adjustable colors [1,2,3,4]. On the whole, it is in line with the current pursuit of low-carbon environmental protection and sustainable scientific development goals [5,6].
At present, using GaInN chips to excite YAG: Ce3+ phosphors is still the most commonly seen solution of commercial lighting [7,8]. However, this scheme has some existing problems, such as high color temperature (CCT), low color rendering index (Ra) and blue-light hazards to the eyes [3]. Therefore, as one way to improve the color rendering ability of white LED, it is of practical significance to develop high-performance red phosphors or seek new excitation resource.
For now, the commercial red phosphor is mainly Y2O3: Eu3+. However, due to its poor thermal stability [9] and invalidity to be excited by near-ultraviolet light [10], new red phosphors doped with Mn4+, Eu3+, Sm3+ and Pr3+ have been extensively explored, such as BaLaMgTaO6: Mn4+ [11], BaMoO4: Eu3+ [12], LiCaGd(WO4)3: Eu3+ [13], Ca2LiScB4O10: Sm3+ [14], Ca3Y(AlO)3(BO3)4: Sm3+ [15], CsMgPO4: Sm3+ [16], Sr3Ga2Sn1.5Si2.5O14: Sm3+ [17], CaTiO3: Pr3+ [18], NaCaTiNbO6: Pr3+ [19].
In a large number of phosphors with different matrix, rare earth doped molybdate has shown a great application potential in red phosphors for w-LED. For example, La2(MoO4)3: Eu3+ [20] phosphors have been found to have good red luminescence properties and an excellent thermal stability; BaY2(MoO4)4: Eu3+ [21] phosphors exhibit a stable red emission with high quantum efficiency; K5La(MoO4)4: Eu3+ [22] phosphors show a high quantum efficiency and potential applications in fingerprint detection. In addition, studies have indicated that the phosphors could present excellent luminescent properties by using non-luminescent centers such as La, Y, and Gd, which have the same valence state and similar ionic radius as the matrix component or co-doped ions [23,24,25]. However, although previous studies have obtained some excellent phosphors, their comprehensive performance is still not good enough, and at the same time, the current theoretical study on the thermal stability of phosphors is not deep enough. It is still of practical significance to prepare excellent red phosphors with high luminous intensity, good thermal stability, high quantum efficiency and high color purity and to enrich their theoretical analysis.
In this work, a series of K5La1-x(MoO4)4: xSm3+ and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Ln3+ (Ln = Sc, Y or Gd) red phosphors were prepared by calcining the mixed raw powders at 600 °C. Meanwhile, the composition and preferable fluorescence properties of the phosphors, especially for the thermal stability, were analyzed in detail.

2. Experimental

2.1. Preparation of the Targets

Firstly, the raw materials including K2CO3(A.R.), La2O3(4N), MoO3(A.R.), Sm2O3(4N), Sc2O3(4N), Y2O3(4N) and Gd2O3(4N) were dried and weighed proportionally in accordance with the designed chemical formula of the phosphors: K5La1-x(MoO4)4: xSm3+ (x = 0.005, 0.01, 0.03, 0.05, 0.07, 0.10, 0.20 and 0.40) and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Ln3+ (Ln = Sc, Y and Gd). After mixed thoroughly in an agate mortar for 20 min, the raw powders were transferred to a corundum crucible and calcined in air at 600 °C for 8 h. Finally, the products were cooled in the furnace and ground to obtain the target samples.

2.2. Characterization of Materials

The X-ray diffraction (XRD) patterns were obtained using Cu-Kα radiation (λ = 1.54056 Å) on the XRD-6000 (Hitachi Japan, Tokyo, Japan) in the range of 10–70° with a scanning step of 0.02°. The XRD results were refined by Rietveld method using GASA software (ver.gasa2full 5455). The microtopography, and the Mapping patterns of the samples were measured by the scanning electron microscope (SEM, JSM-7500, Tokyo, Japan) equipped with INCA X-Max50 (Oxford, UK). The excitation and emission spectra of the samples at different temperature were characterized using Hitachi F-4600 (Chiyoda, Tokyo, Japan) and its heating accessories (Orient KOJI TAP-02, Tianjing, China). The fluorescence lifetime and quantum efficiency of the samples were determined by FluoLog-3 (Horiba Scientific, Kyoto, Japan). The thermoluminescence (TL) spectra of the samples were recorded on TOSL-3DS (Guangzhou, China).

3. Result and Discussion

3.1. Phase Composition and Morphology

Figure 1a demonstrates the XRD patterns of K5La1-x(MoO4)4: xSm3+ phosphors. As can be seen, all the locations and relative intensities of diffraction peaks fit well with the PDF card (#027-1363), and no other obvious secondary phases can be found, indicating that K5La(MoO4)4-based phosphors are successfully prepared without preferential growth. The K5La(MoO4)4 crystal belongs to the trigonal system with space group of R3m, where the La site is surrounded by eight oxygen atoms, forming the [La/K1]O8 octahedral structure (Figure S1). It is worth noting that since the radius of Sm3+ ion is smaller than that of La3+ ion, the peaks slightly shift to a larger angle with the increase of doping concentration. Figure 1b shows the refined XRD patterns of K5La0.93(MoO4)4: 0.07Sm3+ phosphors, from which it can be found the calculation result is in good agreement with the experimental data, the Rp and Rwp are 9.13% and 7.39%, respectively. The information of atomic occupancy obtained from the refinement is listed in Table 1.
Figure 2 presents the SEM microtopography (a) and particle size distribution (b) of K5La0.93(MoO4)4: 0.07Sm3+ phosphors. According to the results of particle size analysis, it is observed that the particle sizes of phosphors are mainly distributed in 5–20 μm, and the average particle size is calculated to be 10.49 μm. It could be seen from the Mapping patterns in Figure S2 that Sm3+ ions in the phosphors sample are uniformly distributed in the matrix.

3.2. Fluorescence Property

Figure 3a displays the excitation and emission spectra of K5La0.93(MoO4)4: 0.07Sm3+ phosphors. Under the monitoring of 600 nm emission, the sample exhibits multiple excitation peaks of 343 nm, 359 nm, 373 nm, 401 nm, 436 nm and 472 nm, which correspond to the 6H2/54K17/2, 4H7/2, 6P7/2, 4F7/2, 4G9/2, and 4I11/2 transitions of Sm3+ ion respectively. Under 401 nm excitation, the phosphors exhibit obvious fluorescence emission peaking at 561 nm, 600 nm and 646 nm, attributed to the 4G5/26H5/2, 6H7/2 and 6H9/2 transitions of Sm3+ ion severally. In addition, a weaker emission peak at 705 nm is observed, ascribed to the 6G2/56H11/2 transition of the Sm3+ ions [26,27].
Figure 3b shows the schematic diagram of the energy levels of Sm3+ ions. After excited, the electrons in the ground state absorb energy and transition to the excited state, and then relax to 4G5/2 through non-radiation (NR). Finally, these electrons transition back to the ground state, emitting the corresponding wavelength of visible light.
Figure 4 exhibits the emission spectra of K5La1-x(MoO4)4: xSm3+ phosphors, and the inset presents the variation trend of the emission intensity at 600 nm (4G5/26H7/2) with doping concentrations (x). Obviously, when the doping concentration is relatively small, the emission intensity of the phosphors is enhanced due to the increase of the luminous centers, reaching a maximum value at x = 0.07, and then concentration quenching occurs.
In general, the concentration quenching mainly takes place in three ways: radiation reabsorption, exchange and multi-dipole interaction [28]. Radiation reabsorption requires obvious overlap between the excitation spectra and emission spectra of phosphors [29], which is not observed in Figure 4, thus radiation reabsorption is not considered. The exchange is a short-range interaction, which plays a role when the critical distance (Rc) of energy transfer between the two neighboring luminous center ions is shorter than 5 Å [30]. The smaller the critical distance, the less probability of concentration quenching. According to Blass’s studies [31,32], Rc can be approximately equal to twice the radius of the sphere in the acting volume:
Rc 2(3V/4πNx)1/3
where V is the volume of unit cell, N is the number of replaceable atoms in the unit cell, and x refers to the critical quenching concentration. According to Formula (1), the Rc of K5La(MoO4)4 matrix is calculated to be 14.30 Å, much longer than 5 Å. In other words, exchange does not contribute to the concentration quenching. Therefore, multi-dipole interaction can be deduced to be responsible for the concentration quenching in K5La(MoO4)4:Sm3+ phosphors.
Dexter’s research [33,34] indicates that the multi-dipole interaction between the luminescent centers in phosphors could be described by the following formula:
log (I/x) = A − θ/3logx
where I stands for the emission intensity, x is the concentration of the luminescent centers, and A is a constant. When θ is equal to 6, 8, 10, it corresponds to dipole-dipole, dipole-quadrupole and quadrupole-quadrupole interaction separately.
Figure 5 exhibits the relationship between lg(I/x) and lg(x) in the K5La1-x(MoO4)4: xSm3+ phosphors according to the Formula (2), which is linearly fitted with the slope (−θ/3) calculated as −1.97, i.e., the θ is equal to 6, indicating the dipole-dipole interaction plays a role.
Figure 6 exhibits the curves of lifetime decay for K5La1-x(MoO4)4:xSm3+ phosphors. Using quadratic exponents to fit the fluorescence lifetime decay curves is a common analytical method [35,36]:
I(t) = I0 + A1 exp(−t/t1) + A2 exp(−t/t2)
In which I0 and I(t) are respectively the initial emission intensity and the emission intensity after the decay time t, A1 and A2 are constants, and the t1 and t2 are two attenuation life factors. Based on this, the average decay life (τ) of the phosphors can be calculated by the following formula [37] and listed in Figure 6:
τ = (A1t12 + A2t22)/(A1t1 + A2t2)
On the whole, the fluorescence lifetime of phosphors decreases with the increase of doping concentration, which might be caused by the interaction or energy transfer between Sm3+ ions [38,39].
As well known, the luminescence properties of rare earth ions are affected by surrounding crystal field environment. In order to further improve the luminescence properties of K5La(MoO4)4: Sm3+ phosphors, Ln3+ (Ln = Sc, Y or Gd) ions are co-doped in K5La0.93(MoO4)4: 0.07Sm3+ phosphors although they do not emit visible light.
As can be seen from Figure S3, the shape and peaking position of XRD patterns do not change significantly after co-doping with Ln3+ ions although deviation of peaks is observed to some different degree, which could be due to the radii difference between Ln3+ ions and La3+ ions, as shown in Table 2, where Dr represents the difference between ions and is calculated by the following formula:
Dr = |(Rm − Rd)/Rm| × 100%
In Formula (5), Rm is the radius of La3+ ions and Rd is the radius of different Ln3+ ions. Studies have demonstrated that when Dr is less than 30%, the dopant ions are more inclined to enter the matrix site in the way of replacement solution [40].
In terms of microtopography, as shown in Figure S4, the co-doping of Ln3+ ions does not significantly change the morphology of phosphors. The Mapping results in Figures S5–S7 further indicate that Ln3+ ions, similar to Sm3+ ions, are uniformly distributed in the phosphors as dopant.
Figure 7 provides the excitation and emission spectra of Ln3+ co-doping phosphors. It can be found that the shape and peaking position of excitation and emission spectra have not changed significantly after co-doping of different Ln3+ ions. However, the emission intensity of phosphors is improved to a certain extent.
Figure 8 shows the change of main emission peaks intensity after Ln3+ ions are co-doped and exhibits its normalization analysis. It can be seen more directly that all the three kinds of Ln3+ ions have either large or small enhancement effects on the three emission peaks intensity. Taking the strongest emission peak of 600 nm as an example, after Sc3+, Y3+ or Gd3+ ions are co-doped, the emission intensity increases to 1.102, 1.055 and 1.387 times of the original value of K5La0.93(MoO4)4: 0.07Sm3+ respectively. Due to the certain ionic radius difference between Ln3+ ions and La3+ ions, the cell would produce a certain degree of contraction, which would enhance the crystal field strength surrounding Sm3+ ions [41]. According to the crystal field theory, the luminescence intensity of rare earth ions would increase with the increase of the crystal field intensity [25,42,43].
According to Table 2, the order of radius difference between Ln3+ ions and La3+ ion is Dr(Sc3+) > Dr(Y3+) > Dr(Gd3+), so the Sc3+ ions co-doped phosphors should have the strongest gain effect. However, the results indicate that the gain effect of Ln3+ ions on phosphors is Gd3+ > Sc3+ > Y3+, which could be explained by the energy transfer between Gd3+ and Sm3+ ions [44,45].
Figure 9 is the schematic diagram of the energy transfer between Gd3+ and Sm3+ ions. Although Sc3+, Y3+ and Gd3+ are all categorized as inert rare earth ions that do not emit light in the visible region [46,47,48], unlike empty filled 4f0 for Sc3+ and Y3+ ions, the 4f electron orbitals of Gd3+(4f7) are half filled, which allows energy transfer through f-f leaps from Gd3+ ions to luminescent center ions [49,50]. In the case of Gd3+ ions being excited, electrons transition from the ground state (8S7/2) to the excited state (6Dj), then relax to the lower energy levels (6IJ, 6Pj) and transfer to the excited states of Sm3+. After further relax to the 4G5/2 level of Sm3+ ions, the electrons eventually transition back to the ground state and emit light. In this way, co-doping of Gd3+ ions increases the number of electrons transitioned from the excited state to the ground state through this energy transfer (ET) process and enhances the luminescence intensity. In order to describe this energy transfer in more detail, we characterized the fluorescence lifetime of K5La0.86(MoO4)4: 0.07(Sm3+, Ln3+) phosphors.
Figure 10 displays the curves of fluorescence lifetime of K5La0.86(MoO4)4: 0.07Sm3+, 0.07Ln3+ (Ln = Sc, Y and Gd) phosphors. It can be seen that the fluorescence lifetime does not change significantly after Sc3+ or Y3+ ions are co-doped, while the fluorescence lifetime of phosphors increases from 1.3971 ms to 1.7027 ms after co-doping of Gd3+ ions. The increase of fluorescence lifetime confirms the energy transfer of Gd3+ ions to Sm3+ ions to some extent [51,52,53].
Figure 11 expresses the emission spectra of K5La0.93(MoO4)4: 0.07Sm3+ (a) and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Gd3+ (b) phosphors, as well as the changes of emission intensity at different temperature (inset). With the increase of temperature, the emission intensity of phosphors first shows a certain enhancement and reaches the highest value at 348 K, and then with the further increase of temperature, although the emission intensity of phosphor gradually decreases, it still keeps at 1.3–1.9 times of the initial emission intensity at 473 K.
In theory, with the increase of temperature, thermal motion of the molecules becomes more active, the phonon action is enhanced, and the probability of the excited electrons returning to the ground state through the form of non-radiative transition increases, eventually the thermal quenching takes place [54]. However, for K5La0.93(MoO4)4: 0.07Sm3+ and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Gd3+ phosphors, the emission intensity increases instead of decreasing, showing an abnormal thermal quenching phenomenon, i.e., zero thermal quenching is found. As a matter of the fact, the thermal stability of a phosphors can be expressed by the thermal activation energy Ea, which can be calculated by the Arrhenius formula below [55]:
ln(I0/I − 1) = lnA − Ea/kT
where I0 and I are the emission intensity at room temperature and T respectively, and k is the Boltzmann constant.
According to the fitting results in Figure 12, the thermal activation energy Ea of K5La0.93(MoO4)4: 0.07Sm3+ and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Gd3+ phosphors is calculated as 0.28 eV and 0.27 eV respectively.
Taken into account the temperature range (298–473 K) of characterization, the possibility of phase transition is little, and far fewer studies reported that Sm3+ ions have thermal coupling energy levels (TCLs) like Dy3+ or Er3+ ions [56,57]. This anomalous thermal quenching phenomenon of the target phosphors might be explained by the electron traps [58,59,60,61].
Figure 13 is a schematic diagram of electron trapping. In general, after excitation, the electrons transition from the ground state to the excited state through the process of ①, then relax to the excited state level with lower energy through ②, and finally return to the ground state via ③ and emit visible light. However, once the electron traps exist in the phosphors, a part of the excited electrons would be captured by them (④) and cannot get enough energy to escape. When the temperature is high enough, these electrons would absorb heat energy and (⑤) escape from the traps to reach the excited state, and finally transition back to the ground state via radiation (⑥). In order to confirm the existence of electron traps in phosphors, the TL spectrum of phosphors are characterized.
Figure 14 is the TL spectrum of the K5La0.93(MoO4)4: 0.07Sm3+ and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Gd3+ phosphors, from which it can be told that the TL spectra have peaks centered at 405 K and 406 K in the range of 300–500 K, at a heating rate of 1 K/s. The appearance of TL peak proves the existence of electron traps to some extent. To better describe the relationship between the electron traps and the TL spectrum, the following two formulas could be used to calculate the depth (Etrap) and density (N0) of the electron traps in the phosphors [35,62]:
Etrap = Tm/500
N0 = ω × Im/{β × [2.52 + 10.2 × (μg − 0.42)]}
In the above formulas, Tm is the temperature corresponding to the highest point of the TL peak, and ω is defined as the shape parameter, ω = τ + δ, in which τ is the low-temperature half-width, and δ is the high temperature half-width. The symmetry parameter μg = δ/(τ + δ), β is the heating rate, and Im is the intensity of the TL peak. According to these formulas, the depth and density of the electron trap in the phosphors are 0.81 eV, 0.812 eV and 2.15 × 106, 2.09 × 106 respectively. The Etrap and N0 of K5La0.93(MoO4)4: 0.07Sm3+ phosphors are slightly larger than that of Gd3+ co-doped phosphors, which is consistent with the thermal stability they exhibit in the illustrations in Figure 11.
Quantum efficiency is another important index to evaluate the performance of phosphors. Figure 15 presents the tested diagram of quantum efficiency of K5La0.86(MoO4)4: 0.07Sm3+, 0.07Gd3+ phosphors. The internal quantum efficiency of phosphors could be calculated from the ratio of the emission to the absorption peak area of the sample [63,64]:
ηq = (∫LS − ∫LB)/(∫EB − ∫ES)
In Formula (9), ∫LS and ∫LB represent the emission spectral area of phosphors and blank sample respectively, while the ∫EB and ∫ES represent the absorption spectral area of phosphors and blank sample. According to Formula (9), the quantum efficiency of K5La0.86(MoO4)4: 0.07Sm3+, 0.07Gd3+ phosphors is calculated to be 74.63%.
Color coordinates are an intuitive representation of the luminous color of the phosphors. Figure 16 displays the color coordinates of the K5La1-x(MoO4)4: xSm3+ and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Ln3+ (Ln = Sc, Y or Gd) (b) phosphors, while Figures S8 and S9 indicate the actual fluorescence photos of these two series of phosphors under ultraviolet irradiation, which suggest the color coordinates of the samples are all located in the orange-red region. Meanwhile, Table 3 and Table 4 list the color coordinates (CIE), color temperature (CCT) and color purity of phosphors samples with different doping concentration, revealing the color temperature of all the phosphors is about 1750–1760 K, and it’s worth noting that the color purity is as high as 99.97%.

4. Conclusions

In this work, a series of K5La1-x(MoO4)4: xSm3+ and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Ln3+ (Ln = Sc, Y or Gd) red phosphors were synthesized via solid state reaction at 600 °C. The excitation and emission spectra of the samples suggest that the phosphors can be efficiently excited at 401 nm and emit visible light at 561 nm, 600 nm and 646 nm, which are corresponding to the 4G5/26Hj/2 (j = 5, 7 and 9) energy transitions of Sm3+ ion with the highest intensity at x = 0.07, and the concentration quenching is attributed to the dipole-dipole interaction. The emission intensity of the phosphors is further improved by co-doping of Ln3+ (Ln = Sc, Y or Gd) ions in the same amount via the enhanced the crystal field strength surrounding Sm3+ ions, among which Gd3+ ions exhibit the best gain effect due to their energy transfer to Sm3+ ions, and the emission intensity is increased by 1.3–1.4 times. It is interesting that K5La1-x(MoO4)4: xSm3+ and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Ln3+ phosphors have excellent thermal stability, even an abnormal thermal quenching phenomenon, i.e., a zero thermal quenching appears. At 473 K, the emission intensity of K5La0.86(MoO4)4:0.07Sm3+, 0.07Gd3+ phosphor is still 1.3–1.8 times that at room temperature, which can be attributed to the electron traps in the phosphors. It is worth mentioning that under 401 nm excitation, the quantum efficiency of the sample is 74.63%. At the same time, the color temperature of the phosphors is 1500–1600 K; and the color purity is as high as 99.97%. These results imply that this red phosphor has potential application in the LED field.

Supplementary Materials

The following supporting information can be downloaded at: https://www.mdpi.com/article/10.3390/inorganics11100406/s1, Figure S1: Schematic diagram of K5La(MoO4)4 crystal structure from different views (a) normal, (b) a axis, (c) b axis, (a) c axis; Figure S2: The Mapping patterns of K5La0.93(MoO4)4: 0.07Sm3+ sample: entirety (a), Mo (b), K (c), O (d), La (e), Sm (f); Figure S3: The XRD pattern of K5La0.86(MoO4)4: 0.07(Sm3+, Ln3+) phosphors; Figure S4: The SEM photos of K5La0.86(MoO4)4: 0.07Sm3+, 0.07Ln3+ (Ln = Sc (a), Y (b) and Gd (c)) phosphors; Figure S5: The EDS and Mapping patterns of K5La0.86(MoO4)4: 0.07(Sm3+, Sc3+) phosphors (inset a-f): Sm (a), Mo (b), K (c), O (d), La (e), Sc (e); Figure S6: The EDS and Mapping patterns of K5La0.86(MoO4)4: 0.07(Sm3+, Y3+) phosphors (insets a-f): Sm (a), Mo (b), K (c), O (d), La (e), Y (e); Figure S7: The EDS and Mapping patterns of K5La0.86(MoO4)4: 0.07(Sm3+, Gd3+) phosphors (insets a-f): Sm (a), Mo (b), K (c), O (d), La (e), Gd (e); Figure S8: Actual fluorescence photos of K5La1-x(MoO4)4: xSm3+, x= 0.005 (a), 0.01 (b), 0.03 (c), 0.05 (d), 0.07 (e), 0.10 (f), 0.20 (g) and 0.40 (h); Figure S9: Actual fluorescence photos of K5La0.86(MoO4)4: 0.07Sm3+, 0.07Ln3+ (Ln = Sc, Y and Gd) phosphors: Sm (a), Sm+Sc (b), Sm+Y(c) and Sm+Gd (d).

Author Contributions

Conceptualization, methodology, T.Z.; validation, T.Z., S.Z. and D.Z.; investigation, S.Z.; resources, D.Z.; data curation, T.Z.; writing—original draft preparation, T.Z.; writing—review and editing, T.Z.; visualization, T.Z.; supervision, D.Z.; project administration, D.Z.; All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Data Availability Statement

The data presented in this study are available on request from the corresponding author.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Fang, M.-H.; Leaño, J.L., Jr.; Liu, R.-S. Control of Narrow-Band Emission in Phosphor Materials for Application in Light-Emitting Diodes. ACS Energy Lett. 2018, 3, 2573–2586. [Google Scholar] [CrossRef]
  2. Wang, L.; Xie, R.J.; Suehiro, T.; Takeda, T.; Hirosaki, N. Down-Conversion Nitride Materials for Solid State Lighting: Recent Advances and Perspectives. Chem. Rev. 2018, 118, 1951–2009. [Google Scholar] [CrossRef]
  3. Ye, S.; Xiao, F.; Pan, Y.X.; Ma, Y.Y.; Zhang, Q.Y. Phosphors in phosphor-converted white light-emitting diodes Recent advances in materials, techniques and properties. Mater. Sci. Eng. R-Rep. 2010, 71, 1–34. [Google Scholar] [CrossRef]
  4. Qiao, J.W.; Zhao, J.; Liu, Q.L.; Xia, Z.G. Recent advances in solid-state LED phosphors with thermally stable luminescence. J. Rare Earths 2019, 37, 565–572. [Google Scholar] [CrossRef]
  5. Schubert, E.F.; Kim, J.K. Solid-state light sources getting smart. Science 2005, 308, 1274–1278. [Google Scholar] [CrossRef]
  6. Pimputkar, S.; Speck, J.S.; DenBaars, S.P.; Nakamura, S. Prospects for LED lighting. Nat. Photonics 2009, 3, 179–181. [Google Scholar] [CrossRef]
  7. Lin, C.C.; Liu, R.S. Advances in Phosphors for Light-emitting Diodes. J. Phys. Chem. Lett. 2011, 2, 1268–1277. [Google Scholar] [CrossRef] [PubMed]
  8. Nathan, M.I. The blue laser diode. GaN based light emitters and lasers. Science 1997, 277, 46–47. [Google Scholar]
  9. Bachmann, V.; Ronda, C.; Meijerink, A. Temperature Quenching of Yellow Ce3+ Luminescence in YAG:Ce. Chem. Mater. 2009, 21, 2077–2084. [Google Scholar] [CrossRef]
  10. McKittrick, J.; Shea-Rohwer, L.E. Review: Down Conversion Materials for Solid-State Lighting. J. Am. Ceram. Soc. 2014, 97, 1327–1352. [Google Scholar] [CrossRef]
  11. Fan, N.S.; Du, Q.; Guo, R.; Luo, L.; Wang, L. Sol-Gel Synthesis and Photoluminescence Properties of a Far-Red Emitting Phosphor BaLaMgTaO6:Mn4+ for Plant Growth LEDs. Materials 2023, 16, 4029. [Google Scholar] [CrossRef]
  12. Li, Z.; Cheng, J.L.; Wang, Y.N.; Wu, K.Y.; Cao, J. Rapid synthesis of BaMoO4:Eu3+ red phosphors using microwave irradiation. Luminescence 2023, 38, 1414–1421. [Google Scholar] [CrossRef]
  13. Wang, D.; Guan, X.F.; Li, G.F. A novel scheelite-type LiCaGd(WO4)3:Eu3+ red phosphors with prominent thermal stability and high quantum efficiency. Int. J. Appl. Ceram. Technol. 2023, 20, 3171–3182. [Google Scholar] [CrossRef]
  14. Sun, G.H.; Chen, Q.L. Novel red-emitting Ca2LiScB4O10: Sm3+phosphor for WLED: Photoluminescence, thermal stability, crystal structure, Judd-Ofelt parameters and energy band gap studies. J. Alloys Compd. 2023, 936, 168263. [Google Scholar] [CrossRef]
  15. Feng, N.N.; Zhang, G.Q.; Bai, S.W.; Lu, D.Z.; Cao, D.Z.; Wu, G.; Han, X.Z.; Wang, F. Sm3+doped Ca3Y(AlO)3(BO3)4: A near-UV pumped orange-red phosphor with high thermal stability. Optik 2023, 275, 170554. [Google Scholar] [CrossRef]
  16. Pradhan, M.K.; Dash, S. Insights into structural and spectroscopic characterization of Sm3+ doped orange rich red emitting CsMgPO4 phosphors. J. Rare Earths 2022, 40, 1837–1848. [Google Scholar] [CrossRef]
  17. Qin, Z.Y.; Dong, L.P.; Zhang, G.H.; Liu, Y.F.; Zhao, G.Y.; Fang, Y.Z.; Hou, J.S. Hetero-valent substitution design of high thermal stability reddish-orange Sr3Ga2Sn1.5Si2.5O14: Sm3+phosphor for healthy lighting white-light-emitting-diodes applications. Opt. Mater. 2022, 131, 112640. [Google Scholar] [CrossRef]
  18. Tian, X.Y.; Wang, C.C.; Wen, J.; Lian, S.X.; Ji, C.Y.; Huang, Z.; Chen, Z.J.; Peng, H.X.; Wang, S.M.; Li, J.; et al. High temperature sensitivity phosphor based on an old material: Red emitting H3BO3 flux assisted CaTiO3: Pr3+. J. Lumin. 2019, 214, 116528. [Google Scholar] [CrossRef]
  19. Xu, D.; Yu, P.L.; Tian, L.H. Luminescence properties of Pr3+ and Bi3+ co-doped NaCaTiNbO6 phosphor for red-LEDs. J. Rare Earths 2018, 36, 243–247. [Google Scholar] [CrossRef]
  20. Ma, Q.C.; Liu, Q.Y.; Wu, M.H.; Liu, Y.F.; Wang, R.; Zhou, R.X.; Xu, Y.H.; Wei, H.C.; Mi, R.Y.; Min, X.; et al. Eu3+-doped La2(MoO4)3 phosphor for achieving accurate temperature measurement and non-contact optical thermometers. Ceram. Int. 2023, 49, 8204–8211. [Google Scholar] [CrossRef]
  21. Krishnan, R.; Kroon, R.E.; Swart, H.C. Charge transfer characteristics and luminescence properties of Eu3+ activated Ba2YMoO6 and BaY2(MoO4)4 phosphors. Mater. Res. Bull. 2022, 145, 111554. [Google Scholar] [CrossRef]
  22. Lin, Y.; He, D.; Jiang, K.; Qin, R.; Wang, J.; Shao, Y.; Yan, J.; Yu, R.; Zhang, D.; Xie, S.; et al. A novel red-emitting K5La(MoO4)4:Eu3+ phosphor with a high quantum efficiency for w-LEDs and visualization of latent fingerprints. J. Alloys Compd. 2023, 960, 170563. [Google Scholar] [CrossRef]
  23. Huang, D.Y.; Ouyang, Q.Y.; Liu, B.; Chen, B.K.; Wang, Y.T.; Yuan, C.G.; Xiao, H.; Lian, H.Z.; Lin, J. Mn2+/Mn4+ co-doped LaM1-xAl11-yO19 (M = Mg, Zn) luminescent materials: Electronic structure, energy transfer and optical thermometric properties. Dalton Trans. 2021, 50, 4651–4662. [Google Scholar] [CrossRef]
  24. Zhao, C.; Zhu, D.C.; Gao, W.; Han, T.; Peng, L.L.; Tu, M.J. Effect of doping Gd3+ on crystal structure and luminescent properties of Sr2SiO4:Eu2+ phosphor. J. Rare Earths 2015, 33, 693–699. [Google Scholar] [CrossRef]
  25. Zhao, C.; Zhu, D.C.; Pu, Y.; Peng, L.L.; Han, T.; Tu, M.J. The effect of doping La3+ on structure and luminescent properties of Sr2SiO4:Eu2+ phosphors. Ceram. Int. 2015, 41, 13341–13347. [Google Scholar] [CrossRef]
  26. Jose, T.A.; Krishnapriya, T.; Jose, A.; C S, R.; Joseph, C.; Biju, P.R. A study on structural and luminescence properties of novel orange-red emitting Sm3+ doped Sr3LiSbO6 nanorod phosphor with high color purity for W-LEDs. J Alloy Compd 2023, 963, 171104. [Google Scholar] [CrossRef]
  27. Lei, B.F.; Li, B.; Zhang, H.R.; Li, W.L. Preparation and luminescence properties of CaSnO3: Sm3+ phosphor emitting in the reddish orange region. Opt. Mater. 2007, 29, 1491–1494. [Google Scholar] [CrossRef]
  28. Niu, P.; Liu, X.; Xie, Z.; Zhao, W. Photoluminescence properties of a novel red-emitting nanowire phosphor Ba6Gd2W3O18:Eu3+. J. Lumin. 2018, 198, 34–39. [Google Scholar] [CrossRef]
  29. Hooda, A.; Khatkar, S.P.; Khatkar, A.; Malik, R.K.; Kumar, M.; Devi, S.; Taxak, V.B. Reddish-orange light emission via combustion synthesized Ba3Y4O9: Sm3+ nanocrystalline phosphor upon near ultraviolet excitation. J. Lumin. 2020, 217, 116806. [Google Scholar] [CrossRef]
  30. Blasse, G. Energy transfer in oxidic phosphors. Phys. Lett. A 1968, 28, 444–445. [Google Scholar] [CrossRef]
  31. Blasse, G. Energy transfer in oxidic phosphors. Philips Res. Rep. 1969, 24, 131. [Google Scholar] [CrossRef]
  32. Li, K.; Chen, D.; Xu, J.; Zhang, R.; Yu, Y.; Wang, Y. Phase transition and multicolor luminescence of Eu2+/Mn2+-activated Ca3(PO4)2 phosphors. Mater. Res. Bull. 2014, 49, 677–681. [Google Scholar] [CrossRef]
  33. Dexter, D.L.; Schulman, J.H. Theory of concentration quenching in inorganic phosphors. J. Chem. Phys. 1954, 22, 1063–1070. [Google Scholar] [CrossRef]
  34. Dexter, D.L. A theory of sensitized luminescence in solids. J. Chem. Phys. 1953, 21, 836–850. [Google Scholar] [CrossRef]
  35. Chen, R. On the calculation of activation energies and frequency factors from glow curves. J. Appl. Phys. 1969, 40, 570–584. [Google Scholar] [CrossRef]
  36. Yang, C.G.; Liu, Y.G.; Yu, H.J.; Liu, Y.K.; Yang, J.Y.; Xie, C.A.; Wang, L.L.; Mi, R.Y. Using energy transfer to obtain warm white-emitting and thermally stable Ca3Y(AlO)3(BO3)4:Dy3+, Eu3+ phosphors. J. Lumin. 2023, 260, 119875. [Google Scholar] [CrossRef]
  37. Monika; Yadav, R.S.; Bahadur, A.; Rai, S.B. 37. Monika; Yadav, R.S.; Bahadur, A.; Rai, S.B. Multicolor tunable bright photoluminescence in Ca2+/Mg2+ modified Eu3+ doped ZnGa2O4 phosphors under UV excitation for solid state lighting applications. RSC Adv. 2023, 13, 20164–20178. [Google Scholar] [CrossRef]
  38. Chen, Y.; Wang, J.; Liu, C.; Kuang, X.; Su, Q. A host sensitized reddish-orange Gd2MoO6:Sm3+ phosphor for light emitting diodes. Appl. Phys. Lett. 2011, 98, 081917. [Google Scholar] [CrossRef]
  39. Martin, J.L.B.; Reid, M.F.; Wells, J.-P.R. Dipole–Quadrupole interactions between Sm3+ ions in KY3F10 nanocrystals. J. Alloys Compd. 2023, 937, 168394. [Google Scholar] [CrossRef]
  40. Pang, R.; Li, C.Y.; Shi, L.L.; Su, Q. A novel blue-emitting long-lasting proyphosphate phosphor Sr2P2O7:Eu2+, Y3+. J. Phys. Chem. Solids 2009, 70, 303–306. [Google Scholar] [CrossRef]
  41. Chen, H.T.; Huang, X.F.; Huang, W.G. Effect of Mn doping on the electronic structure and absorption spectrum of Ba2SiO4:Eu2+ phosphor. Chin. J. Phys. 2016, 54, 931–939. [Google Scholar] [CrossRef]
  42. Gao, X.; Zhang, W.T.; Wang, X.M.; Huang, X.; Du, H.Y.; Lin, J.H. Enhancing the photoluminescence performance of Ca5(PO4)2SiO4:Re3+ (Re = Eu, Sm) phosphors with A(3+) (A = La, Bi) codoping and white light-emitting diode application. Ceram. Int. 2022, 48, 13080–13089. [Google Scholar] [CrossRef]
  43. Yang, L.X.; Wang, J.S.; Zhu, D.C.; Pu, Y.; Zhao, C.; Han, T. The effect of doping Mg2+ on structure and properties of Sr1.992-xMgxSiO4: 0.008Eu2+ blue phosphor synthesized by co-precipitation method. Opt. Mater. 2018, 75, 887–892. [Google Scholar] [CrossRef]
  44. Ullah, I.; Sarumaha, C.S.; Angnanon, A.; Khan, I.; Shoaib, M.; Khattak, S.A.; Kothan, S.; Sangwaranatee, N.; Rooh, G.; Kaewkhao, J. Spectral features of Gd2O3 modified Sm3+doped lithium strontium borate glasses for solid-state laser applications. Ceram. Int. 2023, 49, 13774–13782. [Google Scholar] [CrossRef]
  45. Xu, C.L.; Strzep, A.; Zhang, Z.H.; Kou, H.M.; Ma, F.K.; Su, L.B. Growth and spectroscopic properties of CaxSr1-xF2: Sm: Gd single crystals. J. Lumin. 2022, 249, 119008. [Google Scholar] [CrossRef]
  46. Luo, L.; Liu, R.H.; Liu, Y.H.; Zhuang, W.D.; Li, Y.F.; Qin, S.W. Enhanced luminescence performances of Mn4+-activated Sr4Al14O25 red phosphors by doping with Sc3+ ions. J. Rare Earths 2021, 39, 380–385. [Google Scholar] [CrossRef]
  47. Hao, J.R.; Cao, L.; Wei, Y.; Yan, C.J.; Li, G.G. Improving photoluminescence and thermal stability of CaSi2O2N2:Eu2+ phosphors by codoping lanthanide ions (Ln = Sc, La, Gd, Yb, Lu). Mater. Lett. 2018, 211, 122–125. [Google Scholar] [CrossRef]
  48. Gu, Y.X.; Zhang, Q.H.; Li, Y.G.; Wang, H.Z.; Xie, R.J. Enhanced emission from CaSi2O2N2:Eu2+ phosphors by doping with Y3+ ions. Mater. Lett. 2009, 63, 1448–1450. [Google Scholar] [CrossRef]
  49. Nanda, S.S.; Nayak, P.; Gupta, S.K.; Rawat, N.S.; Goutam, U.K.; Dash, S. Structural, optical spectroscopy and energy transfer features of Tb3+-activated (Y, Gd)F3 nanophosphors for UV-based LEDs. New J. Chem. 2022, 46, 15617–15627. [Google Scholar] [CrossRef]
  50. Ullah, I.; Rooh, G.; Khattak, S.A.; Khan, I.; Shoaib, M.; Kothan, S.; Srisittipokakun, N.; Kaewkhao, J. Spectral characteristics and energy transfer in Gd3+and Nd3+ doped borate glasses for NIR laser applications. Infrared Phys. Technol. 2022, 125, 104272. [Google Scholar] [CrossRef]
  51. Lv, P.; Fang, L.Z.; Xia, H.P.; Song, H.W.; Chen, B.J. The effect of GdF3 on red emission of Eu3+: LiYF4 single crystals grown by the Bridgman method. J. Mater. Sci.-Mater. Electron. 2022, 33, 21628–21637. [Google Scholar] [CrossRef]
  52. Kumar, K.N.; Vijayalakshmi, L.; Kim, J.S. Enhanced red luminescence quantum yield from Gd3+/Eu3+: CaLa2ZnO5 phosphor spheres for photonic applications. Mater. Res. Bull. 2018, 103, 234–241. [Google Scholar] [CrossRef]
  53. Zhou, L.; Tanner, P.A.; Ning, L.; Zhou, W.; Liang, H.; Zheng, L. Spectral Properties and Energy Transfer between Ce3+ and Yb3+ in the Ca3Sc2Si3O12 Host: Is It an Electron Transfer Mechanism? J. Phys. Chem. A 2016, 120, 5539–5548. [Google Scholar] [CrossRef]
  54. Qin, X.; Liu, X.W.; Huang, W.; Bettinelli, M.; Liu, X.G. Lanthanide-Activated Phosphors Based on 4f-5d Optical Transitions: Theoretical and Experimental Aspects. Chem. Rev. 2017, 117, 4488–4527. [Google Scholar] [CrossRef]
  55. Fu, A.J.; Pang, Q.; Yang, H.; Zhou, L.Y. Ba2YNbO6:Mn4+-based red phosphor for warm white light-emitting diodes (WLEDs): Photoluminescent and thermal characteristics. Opt. Mater. 2017, 70, 144–152. [Google Scholar] [CrossRef]
  56. Cao, Z.; Zhou, S.; Jiang, G.; Chen, Y.; Duan, C.; Yin, M. Temperature dependent luminescence of Dy3+ doped BaYF5 nanoparticles for optical thermometry. Curr. Appl. Phys. 2014, 14, 1067–1071. [Google Scholar] [CrossRef]
  57. Liu, S.F.; Ming, H.; Cui, J.; Liu, S.B.; You, W.X.; Ye, X.Y.; Yang, Y.M.; Nie, H.P.; Wang, R.X. Color-Tunable Upconversion Luminescence and Multiple Temperature Sensing and Optical Heating Properties of Ba3Y4O9:Er3+/Yb3+ Phosphors. J. Phys. Chem. C 2018, 122, 16289–16303. [Google Scholar] [CrossRef]
  58. Zhong, Y.; Xia, M.; Chen, Z.; Gao, P.X.; Hintzen, H.T.; Wong, W.Y.; Wang, J.; Zhou, Z. Pyrophosphate Phosphor Solid Solution with High Quantum Efficiency and Thermal Stability for Efficient LED Lighting. Iscience 2020, 23, 100892. [Google Scholar] [CrossRef]
  59. Qian, Y.; Zhu, D.; Pu, Y. A zero-thermal-quenching phosphor Sr3La(AlO)3(BO3)4: Dy3+ for near ultraviolet excitation white-LEDs. J. Lumin. 2022, 243, 118610. [Google Scholar] [CrossRef]
  60. Garlick, G.F.J.; Gibson, A.F. The Electron Trap Mechanism of Luminescence in Sulphide and Silicate Phosphors. Proc. Phys. Soc. Lond. 1948, 60, 574–590. [Google Scholar] [CrossRef]
  61. Geng, X.; Xie, Y.; Chen, S.N.; Luo, J.M.; Li, S.C.; Wang, T.; Zhao, S.C.; Wang, H.; Deng, B.; Yu, R.J.; et al. Enhanced local symmetry achieved zero-thermal-quenching luminescence characteristic in the Ca2InSbO6:Sm3+ phosphors for w-LEDs. Chem. Eng. J. 2021, 410, 128396. [Google Scholar] [CrossRef]
  62. Van den Eeckhout, K.; Smet, P.F.; Poelman, D. Persistent Luminescence in Eu2+-Doped Compounds: A Review. Materials 2010, 3, 2536–2566. [Google Scholar] [CrossRef]
  63. Miao, S.H.; Liang, Y.J.; Shi, R.Q.; Wang, W.L.; Li, Y.F.; Wang, X.J. Broadband Short-Wave Infrared-Emitting MgGa2O4:Cr3+, Ni2+ Phosphor with Near-Unity Internal Quantum Efficiency and High Thermal Stability for Light-Emitting Diode Applications. Acs Appl. Mater. Interfaces 2023, 15, 32580–32588. [Google Scholar] [CrossRef] [PubMed]
  64. Xie, J.H.; Tian, J.H.; Zhuang, W.D. Near-Infrared LuCa2ScZrGa2GeO12:Cr3+ Garnet Phosphor with Ultra-broadband Emission for NIR LED Applications. Inorg. Chem. 2023, 62, 10772–10779. [Google Scholar] [CrossRef]
Figure 1. The XRD patterns of K5La1-x(MoO4)4: xSm3+ phosphors (a), and the refinement pattern of K5La0.93(MoO4)4: 0.07Sm3+ phosphors (b).
Figure 1. The XRD patterns of K5La1-x(MoO4)4: xSm3+ phosphors (a), and the refinement pattern of K5La0.93(MoO4)4: 0.07Sm3+ phosphors (b).
Inorganics 11 00406 g001
Figure 2. The SEM microtopography (a) and particle size distribution (b) of K5La0.93(MoO4)4: 0.07Sm3+ phosphors.
Figure 2. The SEM microtopography (a) and particle size distribution (b) of K5La0.93(MoO4)4: 0.07Sm3+ phosphors.
Inorganics 11 00406 g002
Figure 3. Excitation (black) and emission (red) spectra of K5La0.93(MoO4)4: 0.07Sm3+ phosphors (a) and energy levels diagram of Sm3+ ion (b).
Figure 3. Excitation (black) and emission (red) spectra of K5La0.93(MoO4)4: 0.07Sm3+ phosphors (a) and energy levels diagram of Sm3+ ion (b).
Inorganics 11 00406 g003
Figure 4. Emission spectra of K5La1-x(MoO4)4: xSm3+ phosphors and the emission intensity at 600 nm change with Sm3+ doping concentrations (x) (inset).
Figure 4. Emission spectra of K5La1-x(MoO4)4: xSm3+ phosphors and the emission intensity at 600 nm change with Sm3+ doping concentrations (x) (inset).
Inorganics 11 00406 g004
Figure 5. The relationship between log(I/x) and log(x) in K5La1-x(MoO4)4: xSm3+ phosphors.
Figure 5. The relationship between log(I/x) and log(x) in K5La1-x(MoO4)4: xSm3+ phosphors.
Inorganics 11 00406 g005
Figure 6. Fluorescence lifetime test results of K5La1-x(MoO4)4: xSm3+ phosphors.
Figure 6. Fluorescence lifetime test results of K5La1-x(MoO4)4: xSm3+ phosphors.
Inorganics 11 00406 g006
Figure 7. The excitation (a) and emission (b) spectra of K5La0.86(MoO4)4: 0.07Sm3+, 0.07Ln3+ (Ln = Sc, Y and Gd) phosphors.
Figure 7. The excitation (a) and emission (b) spectra of K5La0.86(MoO4)4: 0.07Sm3+, 0.07Ln3+ (Ln = Sc, Y and Gd) phosphors.
Inorganics 11 00406 g007
Figure 8. The effect of Ln3+ ions co-doping on the intensity of emission peaks (a) and the normalized intensity of main emission peaks (b) after Ln3+ ions co-doping.
Figure 8. The effect of Ln3+ ions co-doping on the intensity of emission peaks (a) and the normalized intensity of main emission peaks (b) after Ln3+ ions co-doping.
Inorganics 11 00406 g008
Figure 9. Energy transfer diagram between Gd3+ and Sm3+ ions.
Figure 9. Energy transfer diagram between Gd3+ and Sm3+ ions.
Inorganics 11 00406 g009
Figure 10. Fluorescence lifetime test results of K5La0.86(MoO4)4: 0.07Sm3+, 0.07Ln3+ (Ln = Sc, Y and Gd) phosphors.
Figure 10. Fluorescence lifetime test results of K5La0.86(MoO4)4: 0.07Sm3+, 0.07Ln3+ (Ln = Sc, Y and Gd) phosphors.
Inorganics 11 00406 g010
Figure 11. Emission spectra at different temperatures of K5La0.93(MoO4)4: 0.07Sm3+ (a) and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Gd3+ (b) phosphors, and the relationship between emission intensity and temperature (insets).
Figure 11. Emission spectra at different temperatures of K5La0.93(MoO4)4: 0.07Sm3+ (a) and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Gd3+ (b) phosphors, and the relationship between emission intensity and temperature (insets).
Inorganics 11 00406 g011
Figure 12. The relationship between ln(I0/I−1) and 1/kT in K5La0.93(MoO4)4: 0.07Sm3+ and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Gd3+ phosphors.
Figure 12. The relationship between ln(I0/I−1) and 1/kT in K5La0.93(MoO4)4: 0.07Sm3+ and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Gd3+ phosphors.
Inorganics 11 00406 g012
Figure 13. Schematic diagram of the electronic traps.
Figure 13. Schematic diagram of the electronic traps.
Inorganics 11 00406 g013
Figure 14. TL spectrum of the K5La0.93(MoO4)4: 0.07Sm3+ and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Gd3+ phosphors.
Figure 14. TL spectrum of the K5La0.93(MoO4)4: 0.07Sm3+ and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Gd3+ phosphors.
Inorganics 11 00406 g014
Figure 15. Quantum efficiency test diagram of K5La0.86(MoO4)4: 0.07Sm3+, 0.07Gd3+ phosphors.
Figure 15. Quantum efficiency test diagram of K5La0.86(MoO4)4: 0.07Sm3+, 0.07Gd3+ phosphors.
Inorganics 11 00406 g015
Figure 16. Color coordinates (CIE) of K5La1-x(MoO4)4: xSm3+ (a) and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Ln3+ (Ln = Sc, Y and Gd) (b) phosphors.
Figure 16. Color coordinates (CIE) of K5La1-x(MoO4)4: xSm3+ (a) and K5La0.86(MoO4)4: 0.07Sm3+, 0.07Ln3+ (Ln = Sc, Y and Gd) (b) phosphors.
Inorganics 11 00406 g016
Table 1. The atomic location parameters of refinement K5La0.93(MoO4)4: 0.07Sm3+.
Table 1. The atomic location parameters of refinement K5La0.93(MoO4)4: 0.07Sm3+.
LabelElemMultxyzFrac
K1K + 130000.418
La1La + 330000.495
Mo1Mo + 66000.4006740.983
K2K + 16000.1950131
O1O − 218−0.0437380.0437380.3186910.262
O2O − 236−0.18550.15090.41730.13
O3O − 218−0.1444550.1444550.4295810.569
Table 2. Comparison of radii between Ln3+ ions and La3+ ion.
Table 2. Comparison of radii between Ln3+ ions and La3+ ion.
CationRadius (Å) (CN = 6)Dr (%)
La3+1.032\
Sm3+0.9587.17
Sc3+0.74527.8
Y3+0.90012.8
Gd3+0.9389.11
Table 3. The CIE, CCT and color purity of K5La1-x(MoO4)4: xSm3+ phosphors.
Table 3. The CIE, CCT and color purity of K5La1-x(MoO4)4: xSm3+ phosphors.
NumberxCIE (xc, yc)CCT (K)Color Purity (%)
10.005(0.5880, 0.4113)176499.97
20.01(0.5888, 0.4105)176199.97
30.03(0.5895, 0.4098)175999.97
40.05(0.5896, 0.4097)175999.97
50.07(0.5898, 0.4095)175899.97
60.10(0.5899, 0.4094)175899.97
70.20(0.5894, 0.4099)175999.97
80.40(0.5870, 0.4123)176799.97
Table 4. The CIE, CCT and color purity of K5La0.86(MoO4)4: 0.07Sm3+, 0.07Ln3+ (Ln = Sc, Y or Gd) phosphors.
Table 4. The CIE, CCT and color purity of K5La0.86(MoO4)4: 0.07Sm3+, 0.07Ln3+ (Ln = Sc, Y or Gd) phosphors.
NumberDopantCIE (xc, yc)CCT (K)Color Purity (%)
10.07Sm3+(0.5898, 0.4095)175899.97
20.07Sm3+ + 0.07Sc3+(0.5922, 0.4071)175399.97
30.07Sm3+ + 0.07Y3+(0.5919, 0.4074)175499.97
40.07Sm3+ + 0.07Gd3+(0.5924, 0.4069)175399.97
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Zhao, T.; Zhang, S.; Zhu, D. A Novel Zero-Thermal-Quenching Red Phosphor with High Quantum Efficiency and Color Purity. Inorganics 2023, 11, 406. https://doi.org/10.3390/inorganics11100406

AMA Style

Zhao T, Zhang S, Zhu D. A Novel Zero-Thermal-Quenching Red Phosphor with High Quantum Efficiency and Color Purity. Inorganics. 2023; 11(10):406. https://doi.org/10.3390/inorganics11100406

Chicago/Turabian Style

Zhao, Tianyang, Shiqi Zhang, and Dachuan Zhu. 2023. "A Novel Zero-Thermal-Quenching Red Phosphor with High Quantum Efficiency and Color Purity" Inorganics 11, no. 10: 406. https://doi.org/10.3390/inorganics11100406

APA Style

Zhao, T., Zhang, S., & Zhu, D. (2023). A Novel Zero-Thermal-Quenching Red Phosphor with High Quantum Efficiency and Color Purity. Inorganics, 11(10), 406. https://doi.org/10.3390/inorganics11100406

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop