Next Article in Journal
Plasma Farming: Non-Thermal Dielectric Barrier Discharge Plasma Technology for Improving the Growth of Soybean Sprouts and Chickens
Next Article in Special Issue
Influence of the On-time on the Ozone Production in Pulsed Dielectric Barrier Discharges
Previous Article in Journal
Cold Atmospheric Pressure Plasma Treatment Modulates Human Monocytes/Macrophages Responsiveness
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

An Inverted Magnetron Operating in HiPIMS Mode

by
Phitsanu Poolcharuansin
1,2,*,
Artit Chingsungnoen
1,2,
Nitisak Pasaja
1,2 and
James W Bradley
3
1
Technological Plasma Research Unit, Department of Physics, Faculty of Science, Mahasarakham University, Maha Sarakham 44150, Thailand
2
Thailand Center of Excellence in Physics, Commission on Higher Education, 328 Si Ayutthaya Road, Bangkok 10400, Thailand
3
Department of Electrical Engineering and Electronics, University of Liverpool, Brownlow Hill, Liverpool L69 3GJ, UK
*
Author to whom correspondence should be addressed.
Plasma 2018, 1(2), 277-284; https://doi.org/10.3390/plasma1020024
Submission received: 1 November 2018 / Revised: 17 November 2018 / Accepted: 26 November 2018 / Published: 27 November 2018
(This article belongs to the Special Issue Latest Developments in Pulsed Low-Temperature Plasmas)

Abstract

:
An ionized physical vapor deposition technique for thin ferromagnetic films is proposed. The technique is based on high power impulse magnetron sputtering (HiPIMS) with positive discharge polarity. A gapped-target was employed as the cathode of the magnetron. By applying positive HiPIMS pulses to the anode, sputtered particles inside the magnetron source were ionized and extracted through the gap. Using a discharge current with a peak of about 13 A, an ion flux in the order of 1021 m−2s−1 was obtained at a distance of 45 mm from the magnetron. In addition, deposition rates of up to 1.1 Å/s for nickel films were achieved using a 30 Hz repetition rate and 300 µs pulse width.

1. Introduction

In conventional magnetron sputtering, energetic electrons are effectively confined due to the presence of transverse magnetic field lines above the target surface. As a consequence, both the ionization rate of the sputtering gas and the sputtering rate of the target material are significantly increased [1].
This is not the case for ferromagnetic metals, e.g., nickel, iron, and cobalt. A ferromagnetic target performs as a magnetic field conductor, completing the magnetic circuit of the magnetron. As a result, most of the magnetic field lines above the target are absent. Therefore, the conventional design of the magnetron is not suitable for the deposition of ferromagnetic films.
Since ferromagnetic thin films are widely used in industrial applications [2,3], a number of magnetron configurations have been proposed that deposit at an acceptable deposition rate [4,5,6,7]. However, the planar Penning trapping configuration [8] is of particular interest here. In this configuration, a circular plate and a concentric ring with a ferromagnetic target are used to form an annular narrow gap. The gap allows some leaking of magnetic field lines and provides the transverse component of the field. The anode cavity below the gap is also introduced to prevent sputtering of the target backing plate.
Recently, the inverted gapped-target magnetron was developed as a device for ferromagnetic film deposition, providing a means to produce good quality, crack-free nickel films [9]. This is mainly due to the ion bombardment with energy of about 200 eV during the film growth. However, the ion density (as implied from the measured discharge current) is rather low when operated in direct current (DC) mode. In addition, the majority of the energetic ions are ionized from the sputtering gas, e.g., argon ions.
High power impulse magnetron sputtering (HiPIMS) is now a well-established technique to generate large ion fluxes of sputtered particles [10]. By applying pulses of high discharge power to a magnetron target, a considerable amount of sputtered species can be ionized by electron-impact ionization in the dense plasma.
The main purpose of the present work was to apply the HiPIMS technique to the inverted magnetron in order to enhance the density of the energetic ions of both gas and metal species. This requires the further modification of a HiPIMS power supply to drive the inverted magnetron with positive pulsed voltages. The discharge characteristics of the magnetron operated in the HiPIMS mode were investigated and are discussed. In addition, the relative deposition rates and ion flux for a number of process conditions were measured using a quartz crystal microbalance (QCM) and a planar electrical probe, respectively.

2. Materials and Methods

The structure of the inverted magnetron has been provided in detail elsewhere [9]. However, a schematic diagram showing the arrangement of the magnetron used in the present work is shown in Figure 1a. The magnetron mainly consisted of a 410-grade stainless-steel anode and a gapped-nickel cathode. The anode was biased to the positive driven-voltage, while the cathode was grounded. The gapped-nickel cathode consisted of two concentric pieces, i.e., a central disk and a ring. The diameter of the central disk was about 31 mm, while the inner and the outer diameter of the ring target was 37 mm and 70 mm, respectively. The thickness of both the central disk and the ring was about 6 mm. Using this target configuration, a complete circular gap was formed with a width of 3 mm. It is important to note that the central disk was actually supported by a target holder held at the axis of the magnetron. However, the holder of the central disk is not shown in Figure 1a for simplicity. The permanent magnets embedded in the anode were employed to generate the magnetic field for the electron confinement at the cathode gap. As a result, the plasma was able to be generated around the cathode gap, enabling the sputtering of cathode material.
Power was supplied to the plasma using a DC pre-ionizer coupled to a HiPIMS unit, in principle, similar to that used in a previous report [11], but with opposite polarity. The DC unit was used to ignite and sustain the background plasma, while the main discharge power was delivered by the HiPIMS unit. The width (w) and repetition rate (f) of the HiPIMS pulse can be adjusted in the range of 20–400 µs and 10–500 Hz, respectively. However, a pulse repetition rate of 30 Hz and a pulse width of 300 µs were selected as the HiPIMS pulse parameters for the present work.
The inverted magnetron was installed in an in-house coating system, as shown in Figure 1b. A cylindrical vacuum chamber was evacuated to a base pressure of 5 × 10−4 Pa by a diffusion pump and a rotary pump. Argon as the sputtering gas was introduced to the chamber via a mass flow controller (4850, Brooks Instrument, Hatfield, PA, country) at a flow rate between 10 sccm and 50 sccm. As a result, the process pressure between 0.3 Pa and 13 Pa could be maintained. In a routine operation, the background plasma is initially ignited at a rather high pressure using the positive DC unit. Then, the argon flow rate is reduced to establish a designed process pressure before applying positive HiPIMS pulses to the magnetron. Using this approach, HiPIMS plasma can be generated during the pulse at pressures down to about 1 Pa.
The waveforms of the discharge voltage (Vd) and current (Id) were measured using a high voltage probe (10076B, Agilent, Santa Clara, CA, USA) and a non-invasive current monitor (101, Pearson Electronics, Palo Alto, CA, USA), respectively. A digital oscilloscope (DSO1002A, Agilent, Santa Clara, CA, USA) were employed for the monitoring and recording of the Vd and Id waveforms. The waveforms of the discharge power (Pd) can be obtained from Pd = VdId.
To investigate the effect of the average discharge power on the particle fluxes arriving at a typical substrate position, probing was performed using: (1) a planar electrical probe to determine the ion flux, and (2) a QCM to determine the sputtered particle arrival rates. The planar probe had a circular stainless steel exposed surface of 16 mm diameter and was grounded to obtain a saturation current (Ip), monitored by a current probe (2877, Pearson Electronics, Palo Alto, CA, USA). Hence, the ion fluxes arriving to the probe could be easily determined. The deposition rate and thickness of the formed nickel films was determined in the vicinity of the flux probe using the QCM devices (STM-2XM, Inficon, Badragaz, Switzerland), both 45 mm from the cathode gap.

3. Results

The discharge waveforms for a process pressure of 1 Pa are shown in Figure 2. In general, the waveforms were almost the same as those of a conventional HiPIMS except for the polarity. In the case of the inverted configuration, the discharge signals were all positive with respect to the ground.
The background plasma, PDC, required a low DC power of about 70 W with a sustained voltage and current of about 230 V and 0.3 A, respectively. The discharge changed to high power mode when a positive pulse from the HiPIMS unit was applied to the anode. Using the initial HiPIMS voltage of 540 V at t = 0 µs, a discharge current of up to a peak (Ipeak) of 13 A developed during the on-time phase (t = 0–300 µs), yielding a peak discharge power (Ppeak) of about 5 kW (see Figure 2a–c). It is worth mentioning that the Vd sharply dropped to below 400 V, corresponding to the high discharge current drawn to the magnetron. The discharge current waveform generally indicates the variation of the plasma density [12]. The discharge current jumped from ~0.3 A in DC mode to ~13 A in HiPIMS mode. The density of the plasma in DC mode has been reported to be approximately 0.6 × 1016 m−3 [9]. Therefore, a plasma density during the HiPIMS pulses in the order of 3 × 1016 m−3 could be expected.
The high discharge current during the HiPIMS pulse agreed well with the probe current determining the ion fluxes at the probe position. The current drawn to the grounded probe is plotted in Figure 3. In the high power mode, an Ip with a peak value of 0.06 A was obtained at the end of the pulse (t ~ 300 µs). It is worth mentioning that a positive current of several hundreds of microamperes was observed even in the DC mode. The positive probe current observed during both the DC and HiPIMS mode indicated that the ion flux arriving to the grounded probe was significantly larger than the electron flux.
It is highly possible that the large ion flux to the grounded probe is mainly due to a high voltage plasma sheath present above the probe surface. The plasma sheath is a layer of electric field formed owing to the potential difference between the plasma potential and the probe potential [13]. Using a Langmuir probe, a plasma potential of larger than 120 V has been estimated in the DC mode [9], causing electron suppression to the grounded probe. Therefore, the electron flux to the probe can be negligible compared to the ion fluxes. In other words, the measured probe current can be used to represent the ion flux (Γi) to the probe as Γi ~ Ip/(qiAp), where qi is the average charge of the ion species (mostly singly charged ions) which is 1.6 × 10−19 C and Ap the probe area.
The corresponding ion flux, calculated from the probe current, is also shown in Figure 3. The ion flux during the HiPIMS pulse dramatically increased to a peak of Γi,peak ~ 1021 m−2s−1. It was two orders of magnitude higher than the ion flux of ~1019 m−2s−1 during the DC mode [9].
Figure 4 shows the peak ion flux Γi,peak determined near the pulse terminal (t ~ 250–300 µs) as a function of the peak of the discharge current Id,peak. It can be seen that the Γi,peak was mostly proportional to the Id,peak, especially in the high current range. The increase of the ion flux mainly contributed to the large discharge current, as well as the discharge power generating the dense plasma during the HiPIMS mode.
The dense plasma increased not only the ion flux but also the sputtered particles. More importantly, the sputtered nickel particles could be effectively ionized in the plasma and could be the major contributor to the thin film deposition process.
Deposition rates (Rd) of nickel films obtained from the QCM reading as a function of the average discharge power (Pd,avg) are shown in Figure 5. It is worth mentioning that the average discharge power was calculated using the equation P d , a v g = f 0 w P d   d t   + P D C . The deposition rate tends to increase with the average HiPIMS power. The maximum deposition rate for the given process condition was about 1.1 Å/s.
In a conventional HiPIMS discharge, during which the negative driving voltage is applied to the target, the plot between the deposition rate and the discharge power density shows a less-than-linear curve [14]. This is due to the returning effect, where the positive metal-ions return to the target, decreasing the deposition rate, particularly at the high discharge power level [15]. This may be not the case for the inverted magnetron. The metal ions created in the inverted magnetron can readily be extracted to the substrate using the positive driving voltage. As a result, a linear deposition rate curve was observed, as seen in Figure 5.
It has been pointed out that the flakes of accumulated film in the magnetron could cause a short-circuit between the cathode and the anode [8]. However, by operating the inverted magnetron in the HiPIMS mode, the amount of the flakes in the magnetron could possibly be reduced, due to ionization and the extraction of the sputtered particles.

4. Discussion

It is reasonable to assume that the discharge mostly occurs inside the magnetron. Therefore, the target surface adjacent to the plasma could be sputtered. In the DC mode, sputtered particles (e.g., Ni) could either be deposited on the anode surface or leave the magnetron through the cathode gap along with the Ar+ ions. In the HiPIMS mode, the plasma density inside the magnetron was expected to be high. Considerable amounts of sputtered particles in the magnetron can be ionized, (e.g., Ni+ and Ni2+), and extracted through the gap forming metal-rich plasma to the substrate.
Using the ion flux probe together with the QCM probe allows us to understand the conceptual idea as follows. The total ion current, obtained from the electrically grounded probe, is proportional to the metal ion flux (Γmi) and gas ion flux (Γgi), written as:
I i Γ m i + Γ g i
Or
I i = q i A p ( Γ m i + Γ g i )
where qi and Ap are the elementary charge on the ion and the probe area, respectively.
In the case of QCM, the deposition rate is proportional to the combination between the metal ion flux (Γmi) and the metal neutral flux (Γmn), written as:
R d ( Γ m i + Γ m n ) ,
Or
R d = K ( Γ m i + Γ m n ) ,
where K is a constant related to the specific process conditions, e.g., the actual density of the depositing film, the target to substrate distance, working pressure, etc.
Since K in Equation (4) is difficult to determine, we focus attention on the relations Equations (1) and (3). The ratio between total ion current, Ii, and deposition rate, Rd, for the HiPIMS mode could be written as:
I i R d ( Γ m i Γ m i + Γ m n ) + ( Γ g i Γ m i + Γ m n ) .
The ratio Ii/Rd is proportional to the summation of two terms. The first term is the ionized metal flux fraction, Θm = Γmi/(Γmi + Γmn) [16]. The second term is the ionized gas flux to total metal flux fraction, Θg = Γgi/(Γmi + Γmn).
Figure 6 shows Ii/Rd as a function of the average discharge power operating in the DC mode and the HiPIMS mode. The ratio of Ii/Rd during the DC mode remains nearly constant. This ratio, however, significantly increases when applying the HiPIMS pulses to the magnetron.
The general trends of Ii/Rd shown in Figure 6 agree well with Equation (5). In the DC mode, the Γmi to the probes can be negligible, owing to the low plasma density. In this case, the Ii/Rd ratio is proportional only to Γgi/Γmn. Even though increasing the DC power may increase both Γgi and Γmn, the measured Ii/Rd ratio is observed to stay nearly constant for the given range of the DC discharge power. In contrast, in the HiPIMS discharge mode with a peak power of a few kW, Γmi and the consequent Θm can significantly increase. This is mainly due to the enhancement of the ionization of nickel atoms in the high density plasma. The ratio of Ii/Rd in the probe position is then observed to increase with the increasing average power.
Operating the magnetron in the HiPIMS mode enhances not only the ionized metal flux fraction Θm at the probe position, but also the density of energetic Ni+ ions (and high ionization states). In our previous work [9], it was shown that the most probable kinetic energy, Em, of ions extracted from the magnetron is closely related to the discharge voltage, Vd. Using the data in [9], we can roughly estimate that Em ~ 0.7qVd (q is the elementary charge). In the present work, Vd during the HiPIMS pulse is about 350 V (see Figure 2a). Therefore, the Em of Ni+ is approximately 240 eV, corresponding to the ion speed of 2.8 × 104 m/s. Using the measured flux of 1.7 × 1021 m−2s−1 (see Figure 3), the density of Ni+ during the HiPIMS pulse was estimated to be approximately 6.0 × 1016 m−3.
Despite the high density of the energetic Ni+ ions, the performance of the gapped magnetron can be discussed as follows. The target gap is similar to the racetrack of the conventional target, where most electrons are effectively confined. In the gapped configuration, the target erosion mostly occurs near the edge of the target gap. We can expect that the gap width will be progressively wider for long-term operation. Furthermore, the discrete erosion may cause an additional instability to the discharge, in particular, when operated in the HiPIMS mode [17]. Further investigation needs to systematically and carefully be performed in order to validate the gapped configuration, both in term of plasma and thin film characterization.

5. Conclusions

An inverted magnetron operating in a high power impulse magnetron sputtering (HiPIMS) mode was proposed. The magnetron is electrically arranged as an inverted magnetron source in which the discharge is sustained using the positive driving voltage. This configuration could provide a large flux of energetic ions, assisting the thin film process. During the positive-voltage HiPIMS pulses, an ion flux in the order of 1021 m−2s−1 and with a density of 6.0 × 1016 m−3 was achieved. Using the ratio between the ion flux and deposition rate, it was interpreted that the ionized metal flux fraction during the HiPIMS mode was significantly higher than that during the DC mode. The linear relationship between the deposition rate and the discharge power indicated little or no back-attraction of ions to the cathode, which is not the case in a conventional HiPIMS.

Author Contributions

Conceptualization, P.P. and J.WB.; methodology, P.P., A.C. and N.P.; formal analysis, P.P., A.C. and N.P.; investigation, P.P., A.C. and N.P.; writing—original draft preparation, P.P.; writing—review and editing, P.P. and J.WB.

Funding

This research was funded by Thailand Center of Excellence in Physics (ThEP) and Faculty of Science, Mahasarakham University, grant number ThEP-61-EQP-MSU2.

Acknowledgments

The authors would like to thank the Integrated Nanotechnology Research Center, Khon Kaen University for technical support of a number of coating equipment.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Abolmasov, S.N. Physics and engineering of crossed-field discharge devices. Plasma Sources Sci. Technol. 2012, 21, 035006. [Google Scholar] [CrossRef]
  2. Howard, J.K. Thin films for magnetic recording technology: A review. J. Vaccum Sci. Technol. A 1986, 4, 1–13. [Google Scholar] [CrossRef]
  3. Qiu, J.; Tang, X.S.; Chen, H.J.; Liu, X.; Hu, Z.W. A tunable broadband magnetoelectric and electromagnetic hybrid vibration energy harvester based on nanocrystalline soft magnetic film. Surf. Coat. Technol. 2017, 320, 447–451. [Google Scholar] [CrossRef]
  4. Keraudy, J.; Delfour-Peyrethon, B.; Ferrec, A.; Molleja, J.G.; Richard-Plouet, M.; Payen, C.; Hamon, J.; Corraze, B.; Goullet, A.; Jouan, P.Y. Process- and optoelectronic-control of NiOx thin films deposited by reactive high power impulse magnetron sputtering. J. Appl. Phys. 2017, 121. [Google Scholar] [CrossRef]
  5. Loch, D.A.L.; Gonzalvo, Y.A.; Ehiasarian, A.P. Nickel coatings by Inductively Coupled Impulse Sputtering (ICIS). Surf. Coat. Technol. 2015, 267, 98–104. [Google Scholar] [CrossRef] [Green Version]
  6. Potocnik, J.; Nenadovic, M.; Bundaleski, N.; Jokic, B.; Mitric, M.; Popovic, M.; Rakocevice, Z. The influence of thickness on magnetic properties of nanostructured nickel thin films obtained by GLAD technique. Mater. Res. Bull. 2016, 84, 455–461. [Google Scholar] [CrossRef]
  7. Caillard, A.; El’Mokh, M.; Semmar, N.; Dussart, R.; Lecas, T.; Thomann, A.L. Energy Transferred From a Hot Nickel Target During Magnetron Sputtering. IEEE Ttrans. Plasma Sci. 2014, 42, 2802–2803. [Google Scholar] [CrossRef]
  8. Window, B.; Sharples, F. Magnetron sputtering sources for ferromagnetic material. J. Vaccum Sci. Technol. A 1985, 3, 10–13. [Google Scholar] [CrossRef]
  9. Poolcharuansin, P.; Laokul, P.; Pasaja, N.; Chingsungnoen, A.; Horprathum, M.; Chindaudom, P.; Bradley, J.W. An inverted gapped-target sputter magnetron for the deposition of thin ferromagnetic films. Vacuum 2017, 141, 41–48. [Google Scholar] [CrossRef]
  10. Gudmundsson, J.T.; Brenning, N.; Lundin, D.; Helmersson, U. High power impulse magnetron sputtering discharge. J. Vaccum Sci. Technol. A 2012, 30, 030801. [Google Scholar] [CrossRef] [Green Version]
  11. Poolcharuansin, P.; Liebig, B.; Bradley, J. Plasma Parameters in a Pre-Ionized HiPIMS Discharge Operating at Low Pressure. IEEE Trans. Plasma Sci. 2010, 38, 3007–3015. [Google Scholar] [CrossRef]
  12. Poolcharuansin, P.; Bradley, J.W. Short- and long-term plasma phenomena in a HiPIMS discharge. Plasma Sources Sci. Technol. 2010, 19, 025010. [Google Scholar] [CrossRef]
  13. Lieberman, M.A.; Lichtenberg, A.J. Principles of Plasma Discharges and Materials Processing; Wiley: Hoboken, NJ, USA, 2005. [Google Scholar]
  14. Hala, M.; Capek, J.; Zabeida, O.; Klemberg-Sapieha, J.E.; Martinu, L. Pulse management in high power pulsed magnetron sputtering of niobium. Surf. Coat. Technol. 2012, 206, 4186–4193. [Google Scholar] [CrossRef]
  15. Anders, A. Deposition rates of high power impulse magnetron sputtering: Physics and economics. J. Vaccum Sci. Technol. A 2010, 28, 783–790. [Google Scholar] [CrossRef]
  16. Poolcharuansin, P.; Bowes, M.; Petty, T.J.; Bradley, J.W. Ionized metal flux fraction measurements in HiPIMS discharges. J. Phys. D Appl. Phys. 2012, 45. [Google Scholar] [CrossRef]
  17. Hecimovic, A.; von Keudell, A. Spokes in high power impulse magnetron sputtering plasmas. J. Phys. D Appl. Phys. 2018, 51. [Google Scholar] [CrossRef]
Figure 1. Schematic diagram of (a) the inverted magnetron and (b) experimental arrangements.
Figure 1. Schematic diagram of (a) the inverted magnetron and (b) experimental arrangements.
Plasma 01 00024 g001
Figure 2. Waveforms of (a) the discharge voltage, (b) the discharge current and (c) the discharge power at the process pressure of 1 Pa. The onset of the pulse is at t = 0 µs.
Figure 2. Waveforms of (a) the discharge voltage, (b) the discharge current and (c) the discharge power at the process pressure of 1 Pa. The onset of the pulse is at t = 0 µs.
Plasma 01 00024 g002
Figure 3. The temporal evolution of the probe current and the corresponding ion flux arriving to the grounded probe.
Figure 3. The temporal evolution of the probe current and the corresponding ion flux arriving to the grounded probe.
Plasma 01 00024 g003
Figure 4. The peak of ion flux Γi,peak as a function of the peak of the discharge current Id,peak.
Figure 4. The peak of ion flux Γi,peak as a function of the peak of the discharge current Id,peak.
Plasma 01 00024 g004
Figure 5. Deposition rate as a function of the discharge power density for 30 Hz with 300 µs pulse parameters.
Figure 5. Deposition rate as a function of the discharge power density for 30 Hz with 300 µs pulse parameters.
Plasma 01 00024 g005
Figure 6. The ratio of the probe current, Ii, to the deposition rate, Rd, as a function of the average discharge power, Pd,avg, delivered to the magnetron.
Figure 6. The ratio of the probe current, Ii, to the deposition rate, Rd, as a function of the average discharge power, Pd,avg, delivered to the magnetron.
Plasma 01 00024 g006

Share and Cite

MDPI and ACS Style

Poolcharuansin, P.; Chingsungnoen, A.; Pasaja, N.; Bradley, J.W. An Inverted Magnetron Operating in HiPIMS Mode. Plasma 2018, 1, 277-284. https://doi.org/10.3390/plasma1020024

AMA Style

Poolcharuansin P, Chingsungnoen A, Pasaja N, Bradley JW. An Inverted Magnetron Operating in HiPIMS Mode. Plasma. 2018; 1(2):277-284. https://doi.org/10.3390/plasma1020024

Chicago/Turabian Style

Poolcharuansin, Phitsanu, Artit Chingsungnoen, Nitisak Pasaja, and James W Bradley. 2018. "An Inverted Magnetron Operating in HiPIMS Mode" Plasma 1, no. 2: 277-284. https://doi.org/10.3390/plasma1020024

APA Style

Poolcharuansin, P., Chingsungnoen, A., Pasaja, N., & Bradley, J. W. (2018). An Inverted Magnetron Operating in HiPIMS Mode. Plasma, 1(2), 277-284. https://doi.org/10.3390/plasma1020024