The Influence of Environment in the Alteration of the Stained-Glass Windows in Portuguese Monuments
Abstract
:1. Introduction
2. Materials and Methods
2.1. Glass Samples
2.2. Corrosion Tests
2.3. Characterization Techniques
3. Results
3.1. Surface Pathologies
3.2. Chemical Alteration
4. Discussion
4.1. Influence of the Glass Composition
4.2. Influence of the Environment
5. Conclusions
Author Contributions
Funding
Acknowledgments
Conflicts of Interest
References
- Hess, D. In search of Luís Alemão. Stained glass in Germany from 1400 till 1460 and the fragments in Batalha. In O Vitral—História, Conservação e Restauro; IPPAR: Lisboa, Portugal, 2000; pp. 44–53. [Google Scholar]
- Ferreira Vieira, S.J. Para a História do Vitral em Portugal no Século XX—As Principais Oficinas e o Papel dos Artistas Plásticos. Master’s Thesis, Faculdade de Ciências Sociais e Humanas, Universidade Nova de Lisboa, Lisboa, Portugal, 2002. [Google Scholar]
- Lopes De Almeida, M. História de S. Domingos by Fr. Luís de Sousa, 1623 (re-edition); Lello e Irmão Editores: Porto, Portugal, 1997. [Google Scholar]
- Woisetschläger, G.; Dutz, M.; Paul, S.; Schreiner, M. Weathering phenomena on naturally weathered potash-lime-silica-glass with Medieval composition studied by Secondary Electron Microscopy and Energy Dispersive Microanalysis. Microchim. Acta 2000, 135, 121–130. [Google Scholar] [CrossRef]
- Munier, I.; Lefèvre, R.; Geotti-Bianchini, F.; Verità, M. Influence of polluted urban atmosphere on the weathering of low durability glasses. Glass Technol. 2002, 43, 225–237. [Google Scholar]
- Lombardo, T.; Lefèvre, R.A.; Chabas, A.; Ausset, P.; Cachier, H.; Ionescu, A. Characterisation of particulate matter deposition inducing soiling of modern glass. In Air Pollution and Cultural Heritage; Saiz-Jimenez, C., Ed.; CRC Press: London, UK, 2004; pp. 209–214. [Google Scholar]
- Melcher, M.; Schreiner, M. Evaluation procedure for leaching studies on naturally weathered potash-lime-silica glasses with medieval composition by scanning electron microscopy. J. Non-Cryst. Solids 2005, 351, 1210–1225. [Google Scholar] [CrossRef]
- Lombardo, T.; Chabas, A.; Lefèvre, R.A.; Ionescu, A. Modelling the soiling of float glass in a polluted atmosphere. Glass Technol. 2005, 46, 192–196. [Google Scholar]
- Vilarigues, M.; Da Silva, R.C. Characterization of potash-glass corrosion in aqueous solution by ion beam and IR spectroscopy. J. Non-Cryst. Solids 2006, 352, 5368–5375. [Google Scholar] [CrossRef]
- Melcher, M.; Schreiner, M. Leaching studies on naturally weathered potash-lime–silica glasses. J. Non-Cryst. Solids 2006, 352, 368–379. [Google Scholar] [CrossRef]
- Favez, O.; Cachier, H.; Chabas, A.; Ausset, P.; Lefevre, R. Crossed optical and chemical evaluations of modern glass soiling in various European urban environments. Atmos. Environ. 2006, 40, 7192–7204. [Google Scholar] [CrossRef]
- Melcher, M.; Schreiner, M.; Kreislova, K. Artificial weathering of model glasses with medieval compositions—An empirical study on the influence of particulates. Phys. Chem. Glasses 2008, 49, 346–356. [Google Scholar]
- Gentaz, L.; Lombardo, T.; Loisel, C.; Chabas, A.; Vallotto, M. Early stage of weathering of medieval-like potash–lime model glass: Evaluation of key factors. Environ. Sci. Pollut. Res. 2011, 18, 291–300. [Google Scholar] [CrossRef] [PubMed]
- Palomar, T. La Interacción de los Vidrios Históricos con Medios Atmosféricos, Acuáticos y Enterramientos. Ph.D. Thesis, Universidad Aunónoma de Madrid, Madrid, Spain, 2013. [Google Scholar]
- Lombardo, T.; Chabas, A.; Verney-Carron, A.; Cachier, H.; Triquet, S.; Darchy, S. Physico-chemical characterisation of glass soiling in rural, urban and industrial environments. Environ. Sci. Pollut. Res. 2014, 21, 9251–9258. [Google Scholar] [CrossRef] [PubMed]
- ICP Materials. International Co-Operative Programme on Effects on Materials Including Historic and Cultural Monuments. Available online: http://www.corr-institute.se/icp-materials/web/page.aspx?sid=3293 (accessed on 15 October 2018).
- Tidblad, J.; Kreislová, K.; Faller, M.; De La Fuente, D.; Yates, T.; Verney-Carron, A.; Grøntoft, T.; Gordon, A.; Hans, U. ICP Materials trends in corrosion, soiling and air pollution (1987–2014). Materials 2017, 10, 969. [Google Scholar] [CrossRef] [PubMed]
- Lombardo, T.; Ionescu, A.; Lefèvre, R.A.; Chabas, A.; Ausset, P.; Cachier, H. Soiling of silica-soda-lime float glass in urban environment: Measurements and modelling. Atmos. Environ. 2005, 39, 989–997. [Google Scholar] [CrossRef]
- Fuchs, D.R.; Römich, H.; Schmidt, H. Glass-Sensors: Assessment of complex corrosive stresses in conservation research. MRS Proc. 2011, 185, 239. [Google Scholar] [CrossRef]
- Leissner, J.; Fuchs, D.R. Investigations by glass sensors on the corrosive environmental conditions at stained glass windows with protective glazings in Europe. MRS Proc. 2011, 267, 1031. [Google Scholar] [CrossRef]
- Basart, S.; Pérez, C.; Cuevas, E.; Baldasano, J.M.; Gobbi, G.P. Aerosol characterization in Northern Africa, Northeastern Atlantic, Mediterranean Basin and Middle East from direct-sun AERONET observations. Atmos. Chem. Phys. 2009, 9, 8265–8282. [Google Scholar] [CrossRef] [Green Version]
- Obregón, M.A.; Pereira, S.; Wagner, F.; Serrano, A.; Cancillo, M.L.; Silva, A.M. Regional differences of column aerosol parameters in western Iberian Peninsula. Atmos. Environ. 2012, 62, 208–219. [Google Scholar] [CrossRef]
- Obregón, M.A.; Serrano, A.; Cancillo, M.L.; Cachorro, V.E.; Toledano, C. Aerosol radiometric properties at Western Spain (Cáceres station). Int. J. Climatol. 2015, 35, 981–990. [Google Scholar] [CrossRef]
- Slezakova, K.; Pereira, M.C.; Reis, M.A.; Alvim-Ferraz, M.C. Influence of traffic emissions on the composition of atmospheric particles of different sizes—Part 1: Concentrations and elemental characterization. J. Atmos. Chem. 2007, 58, 55–68. [Google Scholar] [CrossRef]
- Almeida, S.M.; Freitas, M.C.; Repolho, C.; Dionísio, I.; Dung, H.M.; Caseiro, A.; Alves, C.; Pio, C.A.; Pacheco, A.M.G. Characterizing air particulate matter composition and sources in Lisbon, Portugal. J. Radioanal. Nucl. Chem. 2009, 281, 215–218. [Google Scholar] [CrossRef]
- Alves, L.C.; Reis, M.A.; Freitas, M.C.; Gouveia, M.A. Elemental analysis of particulate matter and source identification in Lisbon. X-ray Spectrom. 1998, 27, 313–320. [Google Scholar] [CrossRef]
- Almeida, S.M.; Pio, C.A.; Freitas, M.C.; Reis, M.A.; Trancoso, M.A. Source apportionment of atmospheric urban aerosol based on weekdays/weekend variability: Evaluation of road re-suspended dust contribution. Atmos. Environ. 2006, 40, 2058–2067. [Google Scholar] [CrossRef]
- Rodrigues, A.; Fearn, S.; Palomar, T.; Vilarigues, M. Early stages of surface alteration of soda-rich-silicate glasses in the museum environment. Corros. Sci. 2018, 143, 362–375. [Google Scholar] [CrossRef]
- Palomar, T.; Chabas, A.; Bastidas, D.M.; De La Fuente, D.; Verney-Carron, A. Effect of marine aerosols on the alteration of silicate glasses. J. Non-Cryst. Solids 2017, 471, 328–337. [Google Scholar] [CrossRef] [Green Version]
- Almeida, R.M.; Pantano, C.G. Structural investigation of silica gel films by infrared spectroscopy. J. Appl. Phys. 1990, 68, 4225–4232. [Google Scholar] [CrossRef]
- Burriel Martí, F.; Lucena Conde, F.; Arribas Jimeno, S.; Hernández Méndez, J. Química Analítica Cualitativa, 18th ed.; Thomson: Madrid, Spain, 2002; ISBN 9788497321402. [Google Scholar]
- Vilarigues, M.; Da Silva, R.C. Ion beam and infrared analysis of medieval stained glass. Appl. Phys. A 2004, 79, 373–378. [Google Scholar] [CrossRef]
- Fernandes, P.; Vilarigues, M.; Alves, L.C.; Da Silva, R.C. Stained glasses from Monastery of Batalha: Non-destructive characterisation of glasses and glass paintings. J. Cult. Herit. 2008, 9, e5–e9. [Google Scholar] [CrossRef]
- Vilarigues, M.; Redol, P.; Machado, A.; Rodrigues, P.A.; Alves, L.C.; Da Silva, R.C. Corrosion of 15th and early 16th century stained glass from the monastery of Batalha studied with external ion beam. Mater. Charact. 2011, 62, 211–217. [Google Scholar] [CrossRef]
- Peel, M.C.; Finlayson, B.L.; Mcmahon, T.A. Updated world map of the Köppen-Geiger climate classification. Hydrol. Earth Syst. Sci. 2007, 11, 1633–1644. [Google Scholar] [CrossRef]
- Iberian Climate Atlas. Air Temperature and Precipitation (1971–2000); Unidad de Documentación de AEMET; Agencia Estatal de Meteorología, Instituto de Meteorologia de Portugal: Madrid, Spain, 2011.
- Kottek, M.; Grieser, J.; Beck, C.; Rudolf, B.; Rubel, F. World Map of the Köppen-Geiger climate classification updated. Meteorol. Z. 2006, 15, 259–263. [Google Scholar] [CrossRef]
- Tullot, I.F. Climatología de España y Portugal; Ediciones Universidad de Salamanca: Salamanca, Spain, 2000; ISSN 84-7800-944-2. [Google Scholar]
- Asay, D.B.; Kim, S.H. Evolution of the adsorbed water layer structure on silicon oxide at room temperature. J. Phys. Chem. B 2005, 109, 16760–16763. [Google Scholar] [CrossRef] [PubMed]
- Gentaz, L.; Lombardo, T.; Chabas, A.; Loisel, C.; Neff, D.; Verney-Carron, A. Role of secondary phases in the scaling of stained glass windows exposed to rain. Corros. Sci. 2016, 109, 206–216. [Google Scholar] [CrossRef]
- Palomar, T.; De La Fuente, D.; Morcillo, M.; Álvarez De Buergo, M.; Vilarigues, M. Early stages of glass alteration in the coastal atmosphere. Build. Environ. 2019, 147, 305–313. [Google Scholar] [CrossRef]
- Carmona, N.; García-Heras, M.; Gil, C.; Villegas, M.A. Chemical degradation of glasses under simulated marine medium. Mater. Chem. Phys. 2005, 94, 92–102. [Google Scholar] [CrossRef]
- Dove, P.M.; Elston, S.F. Dissolution kinetics of quartz in sodium chloride solutions: Analysis of existing data and a rate model for 25 °C. Geochim. Cosmochim. Acta 1992, 56, 4147–4156. [Google Scholar] [CrossRef]
- Palomar, T.; Llorente, I. Decay processes of silicate glasses in river and marine aquatic environments. J. Non-Cryst. Solids 2016, 449, 20–28. [Google Scholar] [CrossRef] [Green Version]
Chemical Composition (wt. %) | ||||||||||||||||
---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
Na2O | MgO | Al2O3 | SiO2 | P2O5 | SO3 | Cl− | K2O | CaO | TiO2 | MnO | Fe2O3 | CuO | ZnO | SnO2 | PbO | |
NCV | 16.91 | 1.77 | 3.15 | 66.12 | 0.02 | 0.03 | 0.01 | 2.86 | 7.30 | 0.03 | 0.09 | 0.27 | - | 1.15 | 0.28 | - |
MCV | 11.70 | 3.43 | 6.81 | 62.97 | 0.12 | - | 0.01 | 4.72 | 8.83 | 0.12 | 0.38 | 0.55 | - | - | 0.38 | - |
KCV | 0.10 | 1.96 | 4.16 | 57.14 | 1.76 | 0.01 | - | 17.56 | 16.64 | 0.06 | - | 0.12 | 0.01 | - | 0.45 | 0.01 |
Lisbon (Caparica Station) | Batalha (Pedrogão Station) | Évora (Évora Station) | ||||
---|---|---|---|---|---|---|
Meteorological Parameters | 10 Months | 20 Months | 10 Months | 20 Months | 10 Months | 20 Months |
Temperature (°C) | 16 ± 5 | 17 ± 5 | 16 ± 6 | - | 17 ± 6 | 18 ± 7 |
26.9 | 20.4 | 31.1 | - | 25.3 | 23.1 | |
16.2 | 10.8 | 18.6 | - | 17.0 | 16.7 | |
Relative Humidity (%) | 72 ± 14 | 71 ± 15 | 69 ± 19 | - | 62 ± 15 | 60 ± 16 |
© 2018 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license (http://creativecommons.org/licenses/by/4.0/).
Share and Cite
Palomar, T.; Redol, P.; Cruz Almeida, I.; Pereira da Silva, E.; Vilarigues, M. The Influence of Environment in the Alteration of the Stained-Glass Windows in Portuguese Monuments. Heritage 2018, 1, 365-376. https://doi.org/10.3390/heritage1020025
Palomar T, Redol P, Cruz Almeida I, Pereira da Silva E, Vilarigues M. The Influence of Environment in the Alteration of the Stained-Glass Windows in Portuguese Monuments. Heritage. 2018; 1(2):365-376. https://doi.org/10.3390/heritage1020025
Chicago/Turabian StylePalomar, Teresa, Pedro Redol, Isabel Cruz Almeida, Eduardo Pereira da Silva, and Marcia Vilarigues. 2018. "The Influence of Environment in the Alteration of the Stained-Glass Windows in Portuguese Monuments" Heritage 1, no. 2: 365-376. https://doi.org/10.3390/heritage1020025
APA StylePalomar, T., Redol, P., Cruz Almeida, I., Pereira da Silva, E., & Vilarigues, M. (2018). The Influence of Environment in the Alteration of the Stained-Glass Windows in Portuguese Monuments. Heritage, 1(2), 365-376. https://doi.org/10.3390/heritage1020025