Next Article in Journal
Effect of Ultrasonic Nanocrystal Surface Modification on the Microstructure and Martensitic Transformation of Selective Laser Melted Nitinol
Previous Article in Journal
Corrosion Inhibition Mechanism and Efficiency Differentiation of Dihydroxybenzene Isomers Towards Aluminum Alloy 5754 in Alkaline Media
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Prediction and Analysis of the Residual Capacity of Concrete-Filled Steel Tube Stub Columns under Axial Compression Subjected to Combined Freeze–Thaw Cycles and Acid Rain Corrosion

1
School of Civil Engineering, Liaoning Technical University, Fuxin 123000, China
2
School of Resource and Civil Engineering, Liaoning Institute of Science and Technology, Benxi 117004, China
3
Transportation and Civil Buildings College, Foshan University, Foshan 528225, China
4
Shaanxi Key Laboratory of Safety and Durability of Concrete Structures, Xi’an 710123, China
5
School of Civil and Environmental Engineering, University of Technology Sydney, Sydney, NSW 2007, Australia
*
Authors to whom correspondence should be addressed.
Materials 2019, 12(19), 3070; https://doi.org/10.3390/ma12193070
Submission received: 30 July 2019 / Revised: 17 September 2019 / Accepted: 18 September 2019 / Published: 20 September 2019
(This article belongs to the Section Construction and Building Materials)

Abstract

:
This paper presents a theoretical investigation on the safety evaluation, stability evaluation, and service life prediction of concrete-filled steel tube (CFST) structures in a Northern China area with acid rain. The finite element software ABAQUS was used to establish a numerical model, which was used to simulate the axial compression behavior of CFST columns subjected to the combined actions of freeze–thaw cycles and acid rain corrosion. The model performance was validated using the experimental results of the evaluation of mechanical properties, including the failure mode and load–displacement curve. Then, the effects of the section size, material strength, steel ratio, and combined times on the residual capacity were studied. The results show that the section size has a smaller influence on the residual strength than the other parameters and can be neglected in the design procedure. However, the other parameters, including the material strength, steel ratio, and combined times have relatively large influences on the axial compressive performance of CFST stub columns subjected to a combination of freeze–thaw cycles and acid rain corrosion. Finally, design formulae for predicting the residual strength of CFST stub columns that are under axial compression and the combined effect of freeze–thaw cycles and acid rain corrosion are proposed, and their results agree well with the numerical results.

1. Introduction

Concrete-filled steel tube (CFST) structures are widely used in real engineering applications in many countries because of their high bearing capacity and good seismic performance [1,2,3,4,5,6,7]. With the rapid development of research and applications, many countries worldwide have promulgated technical specifications for CFST structures [8,9,10,11,12,13]. To date, the main research in this area has focused on the static performance [14,15,16,17], seismic performance [18,19,20], and fire resistance [21,22] of CFST structures, including studies on their structural durability after acid rain corrosion [23] and freeze–thaw cycles [24]. However, previous research on the durability of CFST structures has been limited to a single environmental factor. Few studies have been conducted on the effects of dual or multiple environmental factors on the mechanical properties of CFST structures. For instance, combined changes in positive and negative temperatures are frequent in Northern China, and structures often suffer from frost damage due to low temperatures in winter [25,26,27]. Additionally, acid rain pollution in summer is becoming increasingly serious in the coastal areas, and it can result in the corrosion of steel structures [28,29]. These problems have greatly affected the mechanical properties of CFST structures that experience freeze–thaw cycles and acid rain corrosion, as well as other environmental factors.
This study aims to develop a theoretical solution to the above problems related to the safety evaluation, stability evaluation, and service life prediction of CFST structures subjected to acid rain in Northern China. First, squared CFST (SCFST) stub columns were selected as the research object. On the basis of modifications to the ultimate stress of the core concrete and the yield strength of the external steel tube, the mechanical behaviors of structures subjected to the combined action of freeze–thaw cycles and acid rain corrosion were analyzed by finite element (FE) modeling. Then, the stress mechanism and parameters that affect the residual bearing capacity, together with the corresponding influence rule, were studied. The outcomes of this research can provide theoretical guidance for the design of CFST structures located in areas with acid rain, which is of great significance to practical engineering applications.
The rest of this paper is organized as follows. Section 2 develops numerical models, and their performances are validated using experimental results from the published literature. In Section 3, the whole process of the load–displacement relationship of the specimen during axial compression is analyzed, including the analyses of the failure mode, load–displacement curve, and bearing capacity. Section 4 analyzes the influences of different parameters on the bearing capacity of the specimen and proposes two design formulae as theoretical references for practical engineering applications. Finally, conclusions are drawn in Section 5.

2. Development and Validation of the Finite Element Model

2.1. Stress–Strain Relationships of Materials

A square CFST column is generally composed of steel and concrete materials. The influence of acid rain includes the corrosion of the exterior steel tube, and corrosion is able to reduce not only the effective thickness but also the mechanical properties of the steel tube. In this study, the stress–strain relationship of the steel was adopted from [30], and this relationship accounts for effects due to the corrosion of the steel tube. Freezing and thawing effects can cause the core concrete to become frozen, which can cause internal cracks and weaken the strength of the column. Accordingly, the uniaxial stress–strain relationship model of core concrete from [24], which considers the effect of freeze–thaw cycles, was used in this study. The relevant mathematical expressions are provided below.
(1) The Stress–Strain Relationship Model of Steel:
σ s = E s e ε s ,                                         ε s ε e A ε s 2 + B ε s + C ,                 ε e < ε s ε e 1 f y e ,                                 ε e 1 < ε s ε e 2 f y e 1 + 0.6 ε s ε e 2 ε e 3 ε e 2 ,         ε e 2 < ε s ε e 3 1.6 f y e ,                                     ε s > ε e 3
εe = 0.8fye/Ese
εe1 = 1.5εe
εe2 = 10εe1
εe3 = 100εe1
A = 0.2fy(εe1εe)2
B = 2e1
C = 0.8fye+e2e
Ese = (1 − 0.955γ)Es
fye = (1 − 1.007γ)fy
γ = ∆t/t
t = t − te
where Es denotes the initial elastic modulus of steel, Ese denotes the effective elastic modulus of corroded steel, fy denotes the initial yield strength of steel, fye denotes the effective yield strength of corroded steel, γ denotes the corrosion rate, ∆t denotes the decreasing value of the wall thickness of the corroded steel tube, t denotes the initial wall thickness of the steel tube, and te denotes the effective wall thickness of the corroded steel tube.
Figure 1 shows the stress–strain relationship of a typical steel tube after it is subjected to acid rain corrosion, as calculated by the model proposed above. The related parameter setting for the numerical simulation is fy = 345 MPa, and the range of γ is 0–50%.
(2) The Stress–Strain Relationship Model of Concrete:
y = 2 x x 2 ,               x 1 x β x 1 η + x , x > 1
x = ε / ε 0
y = σ / σ 0
σ 0 = f c 1 0.065 N ft / 100
ε 0 = 1300 + 12.5 f c + 800 ζ e 0.2 × 10 6
η = 1.6 + 1.5 / x
β = f c 0.1 / 1.2 1 + ζ e
f c = 0.76 + 0.2 + log 10 f c u 19.6 f cu
ζ e = α e f ye / f ck
f ck = 0.88 × 0.76 × f cu
α e = A se / A c
E c = 4700 f c )
ψ = 56.3 1 ζ e ,     ζ e 0.5 6.672 e 7.4 4.64 + ζ e ,     ζ e > 0.5
K c = 5.5 5 + 2 f c 0.075
f b 0 / f c 0 = 1.5 f c 0.075
where σ0 and ε0 denote the peak stress and peak strain of the stress–strain relationship of concrete, respectively; fc′ denotes the cylinder compressive strength of concrete; fcu denotes the cube compressive strength of concrete; fck denotes the standard value of the axial compressive strength of concrete; ξe denotes the effective restraint coefficient of CFST; αe denotes the effective steel ratio of the steel tube; Ase denotes the effective area of the steel tube; Ac denotes the area of a concrete section; and Nft denotes the number of freeze–thaw cycles.
Figure 2 shows the typical stress–strain relationship of core concrete after it is subjected to freeze–thaw cycles. The corresponding numerical parameters are fcu = 40 MPa, ζe = 1.0, and the range of Nft is 0–500.
In this study, the Poisson’s ratio of concrete was set to 0.2. The elastic modulus of concrete (Ec), dilation angle (ψ), the ratio of the second stress invariant on the tensile meridian to that on the compressive meridian (Kc), and the ratio of the initial biaxial compressive yield stress to the initial uniaxial compressive yield stress (fb0/fc0) were set according to the corresponding parameter values in [31]. The relevant equations are
E c = 4700 f c
ψ = 56.3 1 ζ e ,     ζ e 0.5 6.672 e 7.4 4.64 + ζ e ,     ζ e > 0.5
K c = 5.5 5 + 2 f c 0.075
f b 0 / f c 0 = 1.5 f c 0.075 .
Furthermore, the eccentricity was set to 0.1, and the viscosity parameter was set to 0.0001 according to [32].

2.2. Numerical Modeling

In this numerical simulation, the FE software ABAQUS 6.13 was employed for modeling and analysis. The steel tube was simulated by the three-dimensional shell element S4R. The Simpson integral method with nine integral points was adopted in the thickness direction of the shell element to ensure calculation accuracy. Concrete was simulated by the three-dimensional solid element C3D8R. Surface-to-surface contact was utilized in the contact mode between the steel tube and concrete. Since the stiffness of the concrete is larger than that of the steel tube, the outer surface of the concrete was set to the main surface, and the inner surface of the steel tube was set to the slave surface. The contact between them was divided into the contacts in the normal direction and tangent direction. In the normal direction, this contact was designated as hard. The tangential friction coefficient was set to 0.6 according to [33]. In the simulation, there was no limit to the contact pressure on the surface between them. For the boundary conditions, one end of the column was set as a fixed constraint to constrain all six degrees of freedom. The other end was loaded with the displacement and only limited in its horizontal leveling ability, which is shown in Figure 3. It is clear that vertical displacement was applied in the U3-direction, with the other two degrees of freedom constrained. Both ends of the model were set as the rigid body to improve the calculation convergence and avoid stress concentration. The geometric center points RP-1 and RP-2 of both ends were taken as reference points. The end corresponding to each reference point was selected as the region type. The calculation cost and accuracy were balanced by taking the mesh size as 1/10 of the width of the cross-section of the column [34]. The meshing and boundary conditions of the FE model are also described in Figure 3.

2.3. Verification of the FE Model

The experimental results of the SCFST members from [24,30,35,36] subjected to the combined action of freeze–thaw cycles and acid rain corrosion were employed to validate the effectiveness of the developed FE model. The detailed analysis and discussion are presented in the following parts.

2.3.1. Experimental Validation of the Freeze–Thaw Cycle Case

(1)
Failure Mode
Figure 4 compares the experimental results in [24,35,36] with the numerical results from the developed FE model. The subfigures show that the failure mode from the numerical analysis results agrees well with that from experimental observation under the same condition. In particular, outward buckling appeared at the end and center of the steel tube, which further validates the effectiveness of the proposed FE model in portraying the failure mode under the freeze–thaw cycle condition.
(2)
Bearing Capacity
The numerical results of the axial bearing capacity of the specimens are provided in Table 1, in which B and t denote the width of the specimen section and the thickness of the steel tube, respectively. Nue denotes the experimental result of the bearing capacity of the specimen; Nce denotes the corresponding bearing capacity simulation result in the literature; and Nbe denotes the result of the bearing capacity of the specimen calculated by the FE model in this study. The comparison results reveal that the prediction errors of Nue/Nbe of almost all the specimens were within ±10%, except for the S3-100, S3-300, S3.9-200, and S3.9-300 specimens. Moreover, the mean value of Nue/Nbe was lower than that of Nue/Nbe; this finding indicates that numerical results of the FE model developed in this study are closer to the corresponding experimental results than the numerical results from the literature. Therefore, it can be concluded that the developed FE model can effectively predict the bearing capacity of SCFST members subjected to freeze–thaw cycles.
(3)
Axial Load–Displacement (or Strain) Curve
Figure 5, Figure 6 and Figure 7 compare the axial load–displacement (or strain) curves between numerical and experimental results. In the figures, the dark yellow dot-dash line denotes the experimental result, the blue dotted line denotes the numerical result from the literature, and the red straight line denotes the numerical result from the FE model developed in this study. It can be observed that the increasing tendencies of the axial load–displacement (or strain) from the numerical results are generally consistent with those from experimental results. However, it is noted that the initial stiffness values of some specimens from the numerical results are different from those of the experimental results. The main reason for this phenomenon is that all the materials were assumed to be in the ideal condition in the numerical simulation. Additionally, measurement error may have resulted in a discrepancy of the initial stiffness. The specimens sometimes had different degrees of initial defects, which could also cause a deviation in the initial stiffness. Furthermore, the descending section of the curves indicates that, compared with the numerical results in the literature, the results calculated from the FE model developed in this study were closer to the experimental values: This sufficiently proves the ability of the proposed model to predict the axial load–displacement (or strain) curves of the specimens subjected to freeze–thaw cycles.

2.3.2. Experimental Validation of the Acid Rain Corrosion Case

In this section, the experimental results for four specimens in [30] are used to verify the developed FE model’s performance in forecasting the ultimate bearing capacity of the specimen subjected to acid rain corrosion. The results of the comparison between the simulation and experimental values of the ultimate bearing capacity are shown in Table 2, in which B and t denote the side length of the specimen section and the initial thickness of the steel tube, respectively; ∆t denotes the reduction value of the wall thickness of the corroded steel tube; γ denotes the corrosion rate; Nue denotes the experimental value of the bearing capacity of the specimens; Nce denotes the corresponding numerical results in [30]; Nbe denotes the numerical results calculated by the developed FE model; and α denotes the initial steel ratio of the specimens. The mathematical expression of α is shown in Equation (32):
α = A s A c
where As and Ac denote the cross-sectional areas of the steel tube and concrete in the initial state, respectively. The comparison results in the table show that the values of Nue/Nbe of all the specimens were less than 5%, which indicates the high prediction accuracy of the developed FE model. For each specimen, the experimental value is closer to the simulation result in this study than the simulation result in the literature. Therefore, it can be concluded that the established FE model is able to accurately predict the mechanical properties of SCFST specimens subjected to acid rain corrosion.

2.3.3. Analysis of Validation Results

The numerical results for the bearing capacity in [24,30,35] were summarized and then compared with the experimental results, as well as the numerical results in this study. Figure 8 shows the comparison result, in which Nue and Nbe denote the simulation results for the bearing capacity from the literature and this study, respectively, and Nce denotes the corresponding experimental results. It is noted that, on the whole, the experimental results are closer to the simulation results of the model developed in this study than the numerical values from the relevant literature. Furthermore, the relative errors between the simulation results in this study and the experimental values were within 20%. Hence, the developed FE model is capable of characterizing the mechanical properties of SCFST stub columns under axial compression and the combined action of freeze–thaw cycles and acid rain corrosion.

3. Whole-Process Analysis of the Load–Displacement Relationship

3.1. Numerical Modeling for Axial Compression

The effect of the combined action of freeze–thaw cycles and acid rain corrosion on the bearing capacity of SCFST stub columns under axial compression was investigated by designing a set of FE models. The calculation parameters of the models are a cross-section width (B) of 400 mm, steel tube thickness (t) of 10 mm, column length (L) of 1200 mm, compressive strength of the concrete cube (fcu) of 40 MPa, yield strength of the steel tube (fy) of 235 MPa, Poisson’s ratios of concrete and steel of 0.2 and 0.3, respectively, and range of the combined frequency of freeze–thaw cycles and acid rain corrosion (p) of 1–5. In the combined process, it was assumed that the freeze–thaw cycles (Nfn = 100) were performed first and that acid rain corrosion (γ = 10%) followed. This process was repeated to realize the combination of freeze–thaw cycles and acid rain corrosion. The detailed parameter values of the developed FE model are listed in Table 3.

3.2. Failure Mode

Figure 9 shows the numerical results for the failure mode of SCFST stub columns subjected to axial loading after suffering different cycles of freeze–thaw and acid rain corrosion. The figure shows that the failure mode of the columns was similar to that of an axially loaded column without any action. Buckling occurred at both ends and in the center of the column. In the real structures, the buckling directions of SCFST columns are all outward. The main reason for this phenomenon is that the inner core concrete of the stub column is capable of providing more effective support to the outer steel tube.
After the SCFST columns experienced different numbers of combined action, the columns were compared. The influence of combination times on the failure mode of the column can be summarized as follows: The larger the combination times, the more serious the local buckling of the steel tube. For the specimen, when the value of p gradually increased from 0 to 5, the peak buckling displacement increased from 0.027 to 0.037 m, which is a percentage increase of 37.04%. The peak value occurred when the value of p was 3. After that, the maximum buckling displacement decreased to 0.035 and 0.032 m, and the values of p were 4 and 5, respectively. Even though the buckling displacement decreased after the combined times exceeded 3, the buckling waves in the center part of the column increased from one to two, which is noticeable in Figure 9f. The main reason for this phenomenon is that the corrosion degree of the steel tube surface was almost the same because the corrosion of the specimens is uniform. When the combined number was small, the corrosion area of the specimen increased with the addition of combined times. Accordingly, there was an increased potential for local defects on the surface of the steel tubes induced by acid rain corrosion, together with the buckling degree at the defect location. Then, as the combined number continued to increase, the corrosion effect of the specimen became more serious, which decreased the effective thickness of the steel tube. Additionally, the buckling displacement also decreased when the steel tube was subjected to axial loading. Since the defect area was enlarged by the increasing corrosion effect, the number of buckling waves also increase.
Figure 10 shows the stress distribution nephogram of the steel tube and core concrete when specimen S-40-235-0.11-3 was axially loaded. Since the specimen was uniformly corroded, the stresses on the four surfaces were approximately the same. Hence, the buckling part of the steel tube and the damaged part of the core concrete were concentrated. For the steel tube, the maximum stress region could be found in the central section of the column, as shown in Figure 10a. The maximum stress at the corner was 252 MPa, which was due to stress concentration. This result indicates that the force for constraining the concrete was the largest at this location. Then, the stress of the steel tube decreased gradually from the central section to both ends along the column height. However, at the ends, the stress slightly increased, and the corresponding value was around 190 MPa. The main reason for this phenomenon is that external constraints in the end region of the column could cause the stress to increase. The longitudinal stress distribution nephogram in the cross-section of the column for the core concrete is depicted in Figure 10b. It is apparent that the maximum stress appeared at the corner of the column with a value of around 26 MPa, followed by the central area with a stress value of around 15 MPa. The minimum stress occurred in the center of the column edge with a value of about 10 MPa. This result indicates that the longitudinal stress distribution of the concrete in the center of the column changed as a result of the constraint effect of the external steel tube.

3.3. Load–Axial Displacement Relationship Curve

Figure 11 shows the relationship between the axial load and displacement of SCFST stub columns after their exposure to freeze–thaw cycles and acid rain corrosion. The combined times of the three curves O–A0–B0–C0–D0, O–A3–B3–C3–D3, and O–A5–B5–C5–D5 were p = 0 (Nft = 0, γ = 0), p = 3 (Nft =300, γ = 30%), and p = 5 (Nft = 550, γ = 50%), respectively. Overall, the increasing tendencies of the load–displacement curves corresponding to different combined times were almost the same. The stress process can be generally divided into four stages: The elastic stage (OAi), the elastic-plastic stage (AiBi), the descending stage (BiCi), and the flat stage (CiDi). A detailed analysis of each stage is reported below.
(1) Elastic Stage (OAi)
In the elastic stage, the relationship between the load and axial displacement is linear. Since the steel tube and concrete work independently, the interaction force between them is 0. Compared with the specimens under the normal condition (without any action, p = 0), the specimens that experience the combined action of freeze–thaw cycles and acid rain corrosion finish the elastic stage early. In addition, with the increase in combined times, the elastic modulus of the specimens gradually decreases, and the elastic phase ends increasingly earlier. This phenomenon is evident in Figure 11b: When p equals 0, the elastic stage is 0-A0; when p equals 3, the elastic stage is 0-A3; and when p equals 5, the elastic stage is 0-A5.
(2) Elastic-Plastic Stage (AiBi)
With the increase in axial load, microcracks in the concrete start to appear and continuously develop. At this stage, the transverse deformation coefficient value of the core concrete is larger than that of the steel tube, and the steel tube has transverse restraint on the core concrete. When the curve arrives at point Bi, the specimens reach their ultimate bearing capacities. Compared with the specimens under the normal condition (without any action, p = 0), the specimens subjected to the combined action of freeze–thaw cycles and acid rain corrosion arrive at point Bi earlier. Furthermore, with the increase in the combination times, the ultimate bearing capacity of the specimen gradually decreases, and the time required to reach the ultimate bearing capacity decreases. When p equals 0, the corresponding ultimate bearing capacity is at point B0; when p equals 3, the corresponding ultimate bearing capacity is at point B3; and when p equals 5, the corresponding ultimate bearing capacity is at point B5.
(3) Descending Stage (BiCi)
After the specimens reach their ultimate bearing capacities, they cease working because of the crushing of the core concrete and the yielding of the steel tube. Finally, the specimens undergo plastic failure. Compared with the specimens under the normal condition (without any action, p = 0), the specimens that experience the combined action of freeze–thaw cycles and acid rain corrosion finish the descending stage earlier and then enter the stable phase. Moreover, with an increase in the combination times, the time required to reach the stable phase decreases. When p equals 0, the corresponding descending endpoint of the specimen is at point C0; when p equals 3, the corresponding descending endpoint of the specimen is at point C3; and when p equals 5, the corresponding descending endpoint of the specimen is at point C5.
(4) Stable Stage (CiDi)
Since the specimens are destroyed, the axial displacements of the specimens rapidly increase. However, regardless of whether the specimens undergo the combined action of freeze–thaw cycles and acid rain corrosion, they have a stable bearing capacity in the later stage, which indicates that the failures of the specimens are plastic failures.

3.4. Bearing Capacity

Figure 12 describes the ultimate bearing capacities of the specimens for different times of combined action of freeze–thaw cycles and acid rain corrosion. It is noted that the ultimate bearing capacity gradually decreased as the combined times increased. Compared with that of the specimen under the normal condition (p = 0), the ultimate bearing capacity of the specimen subjected to the combined action was reduced by 11.4%, 22.4%, 32.9%, 42.1%, and 51.0% when p equaled 1, 2, 3, 4, and 5, respectively. This result sufficiently shows that the combined actions of freeze–thaw cycles and acid rain corrosion have a significant influence on the ultimate bearing capacity of SCFST columns.

3.5. Interaction between the Steel Tube and Core Concrete

The normal contact stress (R)–axial displacement (Δ) relationship between the steel tube and the core concrete of the SCFST stub column is illustrated in Figure 13, in which the normal contact stress is measured at the corner of the section along the center of the column height. The figure indicates that when the axial displacement is initially applied, both the steel tube and core concrete are in the elastic working state. Because the Poisson’s ratio of the steel is larger than that of the concrete, the transverse deformation of the steel is larger than that of the concrete. Because of the gap between the steel tube and core concrete, the normal contact stress between them is zero. As the axial displacement continues to grow, the concrete begins to enter the elastic-plastic working state, and microcracks emerge on the surface of the concrete. In this case, the Poisson’s ratio of the concrete increases more quickly than that of the steel tube. When the transverse deformation of the concrete is larger than that of the steel tube, the normal contact stress between them is generated. With the increase in external load, the normal contact stress gradually rises. As the axial displacement continues to grow, the cracks in the core concrete continue to develop, and the specimen reaches its ultimate bearing capacity. At this time, the concrete surface is cracked and peeled off, the local buckling of the steel tube increases, and the normal contact stress gradually decreases. As the ultimate bearing capacity of the specimen gradually decreases, the axial displacement continues to increase, the core concrete is crushed, and the corresponding transverse deformation rapidly expands. At this point, the external steel enters the strengthening stage, and the restraint effect of the steel tube on the core concrete is enhanced. As a consequence, the normal contact stress between the steel tube and core concrete starts to increase. As observed in the figure, with the increase in combined times, the starting time of the interaction between the steel tube and core concrete becomes progressively earlier. The main reason for this phenomenon is that the more the core concrete is affected by the freeze–thaw cycles, the more the strength decreases, the greater the occurrence of surface cracks, and, thus, the earlier the specimen enters the plastic working stage. With the increase in combined times, the normal contact stress between the steel tube and concrete decreases gradually.

4. Parameter Analysis and Design Method of Bearing Capacity

According to [37], the parameter Ks is defined as the influence factor of the bearing capacity of SCFST columns after axial compression and exposure to the combined action of freeze–thaw cycles and acid rain corrosion. The detailed mathematical expression is given in Equation (33).
K s = N n N 0
where Nn denotes the ultimate bearing capacity of the specimen subjected to the combined action of freeze–thaw cycles and acid rain corrosion, and N0 denotes the ultimate bearing capacity of the specimen under the normal condition.

4.1. Parameter Analysis

In this section, the developed FE model is used to analyze the effects of the section size (B), steel ratio (α), cubic compressive strength of concrete (fcu), yield strength of the steel tube (fy), and combined times (p) on the influence factor Ks. In order to facilitate the parameter analysis and propose the design method, it was assumed that a whole combination (p) consists of freeze–thaw cycles (Nft = 100) and acid rain corrosion (γ = 10%). The mathematical relationship between p, Nft, and γ is provided in Equations (34) and (35). The basic parameters of the specimen were set to B × t × L = 400 × 10 × 1200 mm, α = 0.11, fcu = 40 MPa, and fy = 235 MPa. The ranges of the calculated parameters were set to B = 200–500 mm, α = 0.07–0.23, fcu = 30–60 MPa, fy = 235–420 MPa, and p = 0–5.
p ,   N f t ,   γ = 0 0 0 1 100 10 % 2 200 20 % 3 300 30 % 4 400 40 % 5 500 50 %
p = 0.00375 N f t   + 6.25 γ
Figure 14 portrays the influences of different parameters on the influence factor Ks. As indicated by the four subfigures, the relationship between Ks and the combination times (p) is approximately linear for all the parameters. With the increase in combination times, the value of Ks decreases, with different decreasing rates corresponding to different parameters. The maximum reduction in Ks can reach as high as 60%. Figure 14a shows the influence of section size (B) on Ks. The four curves, which correspond to different values of B, almost overlap, which indicates that the width of the cross-section has little effect on Ks. Figure 14b,c demonstrates the influences of the cubic compressive strength of concrete (fcu) and the yield strength of the steel tube (fy) on the value of Ks, respectively. With the increase in combination times, the descending rates of the curves corresponding to different parameter values differ. Compared with B, fcu and fy have large influences on Ks and can be considered the main factors. Notably, after experiencing the same combined times, the larger the value of fy or the smaller the value of fcu, the smaller the value of Ks. For instance, in the analysis range, when p equaled 3, the value of fy increased from 235 to 420 MPa and the value of Ks decreased from 0.671 to 0.640. When the value of fcu decreased from 60 to 30 MPa, the value of Ks decreased from 0.732 to 0.671. Figure 14d depicts the influence of the steel ratio (α) on Ks. Similar to fcu and fy, α has a significant influence on Ks and is also a major factor. In particular, for the same combination times, the higher the value of α, the faster the decrease in the value of Ks. For example, when p equaled 3, the value of α increased from 0.07 to 0.23 and the value of Ks decreased from 0.716 to 0.575. The main reason for this result is that the steel tube contributes more to the bearing capacity of the specimen than to the core concrete. Consequently, when the thickness and strength of the steel tube are reduced as a result of acid rain corrosion, the influence factor Ks of the residual bearing capacity of the specimens significantly decreases. According to the definition of the constraint effect coefficient ζ, whose mathematical expression is given in Equation (36), if the values of α and fy are larger and the value of fcu is smaller, then the value of Ks is smaller. As a result, it can be concluded that the main factor that affects Ks is ζ.
ζ = α · f y f c u

4.2. Design Formulae

According to the parameter analysis result in Section 4.1, the parameters ζ and p are the main factors affecting Ks. The influence of ζ on Ks is clearly illustrated in Figure 15, in which the value of ζ ranges from 0.59 to 2.06. Hence, the mathematical relationship between Ks, ζ, and p can be obtained by using the regression method. According to the commonly used parameter ranges in a practical engineering application, the ranges of ζ and p are [0.5, 2] and [0, 5], respectively. Figure 15 shows that the relationships between Ks and p for different values of ζ are approximately linear. Accordingly, the following mathematical expression can be obtained:
K s = 1 + k · p
where k is the function of ζ. From the numerical results, a simplified formula for Ks can be obtained as follows.
K s = 1.08 0.0667 ζ 0.105 p
Currently, the specification GB50936-2014 [8] is commonly used to calculate the bearing capacity of SCFST stub columns in China. The formula for calculating the bearing capacity of SCFST stub columns under axial compression in the specification is given below:
N0 = (1.212 + + 2) Asc fck
B1 = 0.131fy/213 + 0.723
C = −0.070fck/14.4 + 0.026
where Asc denotes the combined cross-section area and B1 and C denote the restraint coefficients of the sectional shape. The substitution of Equations (38)–(41) into Equation (33) results in the equation for the residual bearing capacity Nn of SCFST stub columns under the combined action of freeze–thaw cycles and acid rain corrosion, as shown in Equation (42):
Nn = (1.08 − 0.0667ζ−0.105p] · [1.212 + (0.131fy/213 + 0.723)ζ + (−0.070fck/14.4 + 0.026)ζ2] Asc fck
where the ranges of the parameters ζ, p, fy, and fck are [0.5, 2], [0, 5], [0, 500], and [20, 40] MPa, respectively.
The accuracy of the proposed simplified design formula based on GB50936-2014 (Equation (42)) was verified by a comparison with the numerical results obtained from the FE model. The comparison is shown in Figure 16a, in which the results of simulating 72 SCFST stub columns under axial compression are compared with those calculated from the proposed design formula based on GB50936-2014 (Equation (42)). Minor discrepancies are observed between the numerical results from the FE model and the calculation results from the proposed design formula based on GB50936-2014. The mean value of Nfn/Ncn for 72 specimens was 1.014, and the corresponding standard deviation was 0.002. The relative errors could be controlled within ±15%.
In addition to the specification GB50936-2014, Eurocode 4 [11] also proposed a design formula for calculating the bearing capacity of a CFST member under axial compression, as provided in Equation (43):
N0 = fy As+ fc′ Ac.
The substitution of Equations (38) and (43) into Equation (33) produces the equation for calculating the residual bearing capacity Nn of SCFST stub columns under the combined action of freeze–thaw cycles and acid rain corrosion:
Nn = (1.08 − 0.0667ζ−0.105p) · (fy As + fc′Ac)
where the ranges of the parameters ζ, p, fy, and fc′ are [0.5, 2], [0, 5], [0, 500], and [24, 51] MPa, respectively.
Similarly, the performance of the developed design formula based on Eurocode 4 was also validated using the numerical results. The evaluation result is shown in Figure 16b, in which the results of simulating 72 SCFST stub columns under axial compression are compared with the results calculated from the proposed design formula based on Eurocode 4 (Equation (44)). Compared with the design formula based on GB50936-2014, the formula based on Eurocode 4 performed better, with a mean value of Nfn/Ncn of 1.007 and a standard deviation of 0.002. Furthermore, the relative errors predicted by Equation (44) could also be controlled within 15%.
Consequently, from the comparison results, it can be proven that both simplified design formulae are capable of predicting the residual bearing capacity of SCFST stub columns that are under axial compression and subjected to the combined action of freeze–thaw cycles and acid rain corrosion. Therefore, the outcome of this study can provide theoretical guidance for the safety evaluation, stability evaluation, and service life prediction of CFST structures in cold and acid rain areas.

5. Conclusions

This study numerically investigated the mechanical properties of the SCFST stub columns that are under axial compression and subjected to the combined action of freeze–thaw cycles and acid rain corrosion. An FE model was established using the software ABAQUS, and the model performance was validated using the experimental data captured from the literature. The effects of different model parameters on the residual capacity were studied, and design formulae were developed to evaluate the residual strength of SCFST stub columns in practice. The detailed conclusions are provided in this section.
(1)
The failure mode of SCFST stub columns subjected to freeze–thaw cycles and acid rain corrosion is similar to that of columns without any action after they are axially loaded. Buckling occurs at both ends and in the central height of the columns. With the increase in the combined times, the local buckling amplitude of the steel tube increases.
(2)
The load–displacement curves of SCFST stub columns under axial compression are basically the same after the columns are subjected to the combined action of freeze–thaw cycles and acid rain corrosion. All the curves include the elastic stage, elastic-plastic stage, descending stage, and stable stage. Under the same conditions, as the combination times increase, the times at which the specimens arrive at each stage are earlier. Regardless of whether the specimens undergo a combination of freeze–thaw cycles and acid rain corrosion, they all have stable bearing capacities in the later stage, and the failure type is a plastic failure.
(3)
The parameters that influence the ultimate bearing capacity of the specimens after freeze–thaw cycles and acid rain corrosion include the restraint effect coefficient (ζe) and combination times (p), which cannot be neglected. Generally, the larger the restraint effect coefficient or the combination times, the smaller the influence factor (Ks) of the residual bearing capacity.
(4)
From the result of parameter analysis, design formulae are proposed for predicting the bearing capacity of the SCFST column that is under axial compression and subjected to the combined action of freeze–thaw cycles and acid rain corrosion.
This paper reports a preliminary investigation into the effects of acid rain corrosion and freeze–thaw cycles on the mechanical properties of SCFST columns from a simplified perspective. Only uniform corrosion was considered in this study. In future work, the durability of CFST structures under local corrosion and freeze–thaw cycles will be analyzed. In addition, the mechanical properties of CFST structures due to other dual environmental factors and even multiple environmental factors will be studied for practical applications. The interdependency of multiple effects should be incorporated into the numerical analysis model to replicate the real-world situation. Related experiments will also be conducted in the laboratory, and the results will be used to further evaluate the effectiveness of the developed numerical model in predicting the mechanical properties of SCFST stub columns that are under axial compression and subjected to the combined action of freeze–thaw cycles and acid rain corrosion.

Author Contributions

Conceptualization, T.Z. and X.L.; methodology, T.Z.; validation, T.Z. and X.L.; writing—original draft preparation, T.Z., X.L., and Y.Y.; writing—review and editing, X.L. and Y.Y.; supervision, X.L. and Y.Y.; project administration, X.L.; funding acquisition, X.L.

Funding

This research was supported by the National Natural Science Foundation of China (Grant Nos. 51208246 and 51808352), Open Fund of Shaanxi Key Laboratory of Safety and Durability of Concrete Structures (XJKFJJ201902), and China Scholarship Council (CSC).

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Hua, Y.X.; Han, L.H.; Wang, Q.L.; Hou, C. Behaviour of square CFST beam-Columns under combined sustained load and corrosion: Experiments. Thin-Walled Struct. 2019, 136, 353–366. [Google Scholar] [CrossRef]
  2. Lyu, X.; Xu, Y.; Xu, Q.; Yu, Y. Axial compression performance of square thin walled concrete-Filled steel tube stub columns with reinforcement stiffener under constant high-Temperature. Materials 2019, 12, 1098. [Google Scholar] [CrossRef] [PubMed]
  3. Yang, Z.; Xu, C. Research on compression behavior of square thin-Walled CFST columns with steel-Bar stiffeners. Appl. Sci. 2018, 8, 1602. [Google Scholar] [CrossRef]
  4. Wu, H.; Cao, W.; Qiao, Q.; Dong, H. Uniaxial compressive constitutive relationship of concrete confined by special-shaped steel tube coupled with multiple cavities. Materials 2016, 9, 86. [Google Scholar] [CrossRef] [PubMed]
  5. Qiao, Q.; Zhang, W.; Qian, Z.; Cao, W.; Liu, W. Experimental study on mechanical behavior of shear connectors of square concrete filled steel tube. Appl. Sci. 2017, 7, 818. [Google Scholar] [CrossRef]
  6. Liu, W.; Cao, W.; Zhang, J.; Wang, R.; Ren, L. Mechanical behavior of recycled aggregate concrete-Filled steel tubular columns before and after fire. Materials 2017, 10, 274. [Google Scholar] [CrossRef]
  7. Li, R.; Yu, Y.; Samali, B.; Li, C. Parametric analysis on the circular CFST column and RBS steel beam joints. Materials 2019, 12, 1535. [Google Scholar] [CrossRef]
  8. Technical Code for Concrete Filled Steel Tubular Structures; GB50936-2014; Ministry of Housing and Urban-Rural Development of the People’s Republic of China (MOHURD): Beijing, China, 2014.
  9. Technical Specification for Structures with Concrete-Filled Rectangular Steel Tube Members; CECS159-2004; China Association for Engineering Construction Standardization: Beijing, China, 2004.
  10. Steel, Concrete and Composite Bridges Part 5: Code of Practice for the Design of Composite Bridges; BS 5400-5:2005; British Standards Institution: London, UK, 2005.
  11. Eurocode 4: Design of Composite Steel and Concrete Structures, Part 1.1. General Rules and Rules for Buildings. EN 1994-1-1; British Standards Institution: London, UK, 2004.
  12. ACI 318-05. Building Code Requirements for Structural Concrete and Commentary; American Concrete Institute: Farmington Hills, MI, USA, 2005. [Google Scholar]
  13. AIJ. Recommendations for Design and Construction of Concrete Filled Steel Tubular Structures; Architectural Institute of Japan: Tokyo, Japan, 2008. [Google Scholar]
  14. Du, Y.; Chen, Z.; Zhang, C.; Cao, X. Research on axial bearing capacity of rectangular concrete-Filled steel tubular columns based on artificial neural networks. Front. Comput. Sci. 2017, 11, 863–873. [Google Scholar] [CrossRef]
  15. Patel, V.I.; Hassanein, M.F.; Thai, H.T.; Al Abadi, H.; Elchalakani, M.; Bai, Y. Ultra-High strength circular short CFST columns: Axisymmetric analysis, behaviour and design. Eng. Struct. 2019, 179, 268–283. [Google Scholar] [CrossRef]
  16. Shams, M.; Saadeghvaziri, M.A. Nonlinear response of concrete-Filled steel tubular columns under axial loading. ACI Struct. J. 1999, 96, 1009–1017. [Google Scholar]
  17. Montuori, R.; Piluso, V. Analysis and modelling of CFT members: Moment curvature analysis. Thin-Walled Struct. 2015, 86, 157–166. [Google Scholar] [CrossRef]
  18. Susantha, K.A.S.; Ge, H.; Usami, T. Cyclic analysis and capacity prediction of concrete-Filled steel box columns. Earthq. Eng. Struct. Dyn. 2002, 31, 195–216. [Google Scholar] [CrossRef]
  19. Wang, X.T.; Xie, C.D.; Lin, L.H.; Li, J. Seismic behavior of self-Centering concrete-Filled square steel tubular (CFST) column base. J. Constr. Steel Res. 2019, 156, 75–85. [Google Scholar] [CrossRef]
  20. Wang, J.; Sun, Q.; Li, J. Experimental study on seismic behavior of high-Strength circular concrete-Filled thin-Walled steel tubular columns. Eng. Struct. 2019, 182, 403–415. [Google Scholar] [CrossRef]
  21. Zhou, K.; Han, L.H. Modelling the behaviour of concrete-Encased concrete-Filled steel tube (CFST) columns subjected to full-Range fire. Eng. Struct. 2019, 183, 265–280. [Google Scholar] [CrossRef]
  22. Yang, H.; Liu, F.; Gardner, L. Post-Fire behaviour of slender reinforced concrete columns confined by circular steel tubes. Thin-Walled Struct. 2015, 87, 12–29. [Google Scholar] [CrossRef]
  23. Yuan, F.; Chen, M.; Huang, H.; Xie, L.; Wang, C. Circular concrete filled steel tubular (CFST) columns under cyclic load and acid rain attack: Test simulation. Thin-Walled Struct. 2018, 122, 90–101. [Google Scholar] [CrossRef]
  24. Yang, Y.F.; Cao, K.; Wang, T.Z. Experimental behavior of CFST stub columns after being exposed to freezing and thawing. Cold Reg. Sci. Technol. 2013, 89, 7–21. [Google Scholar] [CrossRef]
  25. Wei, H.; Wu, Z.; Guo, X.; Yi, F. Experimental study on partially deteriorated strength concrete columns confined with CFRP. Eng. Struct. 2009, 31, 2495–2505. [Google Scholar] [CrossRef]
  26. Qin, Z.; Lai, Y.; Tian, Y.; Yu, F. Frost-Heaving mechanical model for concrete face slabs of earthen dams in cold regions. Cold Reg. Sci. Technol. 2019, 161, 91–98. [Google Scholar] [CrossRef]
  27. Zhang, G.; Yu, H.; Li, H.; Yang, Y. Experimental study of deformation of early age concrete suffering from frost damage. Constr. Build. Mater. 2019, 215, 410–421. [Google Scholar] [CrossRef]
  28. Zhang, X.; Jiang, H.; Zhang, Q.; Zhang, X. Chemical characteristics of rainwater in northeast China, a case study of Dalian. Atmos. Res. 2012, 116, 151–160. [Google Scholar] [CrossRef]
  29. Liu, M.; Song, Y.; Zhou, T.; Xu, Z.; Yan, C.; Zheng, M.; Wu, Z.; Hu, M.; Wu, Y.; Zhu, T. Fine particle pH during severe haze episodes in northern China. Geophys. Res. Lett. 2017, 44, 5213–5221. [Google Scholar] [CrossRef]
  30. Cheng, M.; Lin, B.; Huang, H. Research on the bearing capacity of corroded square concrete filled steel tubular short column. Steel Constr. 2017, 32, 110–116. [Google Scholar]
  31. Tao, Z.; Wang, Z.B.; Yu, Q. Finite element modelling of concrete-filled steel stub columns under axial compression. J. Constr. Steel Res. 2013, 89, 121–131. [Google Scholar] [CrossRef]
  32. Tian, J. Behavior of Eccentricity Loaded Circular Stainless Steel-Carbon Steel Composite Tube Confined Concrete Columns. Ph.D. Thesis, Harbin Institute of Technology, Harbin, China, 2017. [Google Scholar]
  33. Han, L.H.; Yao, G.H.; Tao, Z. Performance of concrete-Filled thin-Walled steel tubes under pure torsion. Thin-Walled Struct. 2007, 45, 24–36. [Google Scholar] [CrossRef]
  34. Zhou, X.; Cheng, G.; Liu, J.; Gan, D.; Frank Chen, Y. Behavior of circular tubed-RC column to RC beam connections under axial compression. J. Constr. Steel Res. 2017, 130, 96–108. [Google Scholar] [CrossRef]
  35. Cao, K. Study on Performance of Concrete-Filled Steel Tubular Stub Columns after being Exposed to Freezing and Thawing. Ph.D. Thesis, Dalian University of Technology, Dalian, China, 2013. [Google Scholar]
  36. Wang, K.; Liu, W.; Chen, Y.; Wang, J.; Xie, Y.; Fang, Y.; Liu, C. Investigation on mechanical behavior of square CFST stub columns after being exposed to freezing and thawing. J. Guangxi Univ. 2017, 42, 1250–1255. [Google Scholar]
  37. Han, L.H.; Hou, C.C.; Wang, Q.L. Behavior of circular CFST stub columns under sustained load and chloride corrosion. J. Constr. Steel Res. 2014, 103, 23–36. [Google Scholar] [CrossRef]
Figure 1. The stress–strain relationship of a steel tube after acid rain corrosion.
Figure 1. The stress–strain relationship of a steel tube after acid rain corrosion.
Materials 12 03070 g001
Figure 2. The stress–strain relationship of core concrete after freeze–thaw cycles.
Figure 2. The stress–strain relationship of core concrete after freeze–thaw cycles.
Materials 12 03070 g002
Figure 3. Finite element model meshing and boundary conditions.
Figure 3. Finite element model meshing and boundary conditions.
Materials 12 03070 g003
Figure 4. Comparison of failure modes between the numerical results and experimental results in the literature. (a) Sc1-300 specimen in [24]; (b) S2-100 specimen in [35]; and (c) SC30-T2.5-N100 specimen in [36].
Figure 4. Comparison of failure modes between the numerical results and experimental results in the literature. (a) Sc1-300 specimen in [24]; (b) S2-100 specimen in [35]; and (c) SC30-T2.5-N100 specimen in [36].
Materials 12 03070 g004
Figure 5. Comparisons between numerical results in this study and the results (both experimental and numerical) in [24].
Figure 5. Comparisons between numerical results in this study and the results (both experimental and numerical) in [24].
Materials 12 03070 g005aMaterials 12 03070 g005b
Figure 6. Comparisons between the numerical results in this study and the results (both experimental and numerical) in [35].
Figure 6. Comparisons between the numerical results in this study and the results (both experimental and numerical) in [35].
Materials 12 03070 g006aMaterials 12 03070 g006b
Figure 7. Comparisons between the numerical results in this study and the experimental results in [36].
Figure 7. Comparisons between the numerical results in this study and the experimental results in [36].
Materials 12 03070 g007aMaterials 12 03070 g007b
Figure 8. Comparisons between experimental and simulation results.
Figure 8. Comparisons between experimental and simulation results.
Materials 12 03070 g008
Figure 9. Failure modes of squared concrete-filled steel tube (SCFST) stub columns with different combined times of actions.
Figure 9. Failure modes of squared concrete-filled steel tube (SCFST) stub columns with different combined times of actions.
Materials 12 03070 g009
Figure 10. Stress distribution nephogram of steel tube and concrete.
Figure 10. Stress distribution nephogram of steel tube and concrete.
Materials 12 03070 g010
Figure 11. Load–axial displacement curve of specimens.
Figure 11. Load–axial displacement curve of specimens.
Materials 12 03070 g011
Figure 12. Influence of combined times on the ultimate bearing capacity of the specimen.
Figure 12. Influence of combined times on the ultimate bearing capacity of the specimen.
Materials 12 03070 g012
Figure 13. The relationship between the normal contact stress and axial displacement.
Figure 13. The relationship between the normal contact stress and axial displacement.
Materials 12 03070 g013
Figure 14. Influences of different parameters on Ks (defined as the influence factor of the bearing capacity of SCFST columns after axial compression and exposure to the combined action of freeze–thaw cycles and acid rain corrosion) of the specimen.
Figure 14. Influences of different parameters on Ks (defined as the influence factor of the bearing capacity of SCFST columns after axial compression and exposure to the combined action of freeze–thaw cycles and acid rain corrosion) of the specimen.
Materials 12 03070 g014
Figure 15. Influence of the constraint effect constraint effect coefficient ζ and combination times p on Ks of the specimen.
Figure 15. Influence of the constraint effect constraint effect coefficient ζ and combination times p on Ks of the specimen.
Materials 12 03070 g015
Figure 16. Comparisons between the simulation results from the finite element (FE) model and the calculation results from design formulae for calculating bearing capacity.
Figure 16. Comparisons between the simulation results from the finite element (FE) model and the calculation results from design formulae for calculating bearing capacity.
Materials 12 03070 g016
Table 1. Bearing capacity comparisons between the numerical results and experimental results of specimens exposed to freeze–thaw cycles.
Table 1. Bearing capacity comparisons between the numerical results and experimental results of specimens exposed to freeze–thaw cycles.
Specimen IDB × t
(mm)
Nue
(kN)
Nce
(kN)
Nbe
(kN)
Nue/NceNue/NbeLiterature Sources
Sc1-50100 × 2.06604.5618.3646.40.9770.934[24]
Sc1-200100 × 2.06606.4580.1614.41.0440.985
Sc1-300100 × 2.06593.7555.7588.11.0681.010
Sc2-50100 × 2.06810.2715.0756.71.1331.064
Sc2-200100 × 2.06803.5668.2750.41.2021.071
Sc2-300100 × 2.06757.0636.7748.21.1891.012
Mean value1.1021.013
Standard deviation0.0080.003
S2-0100 × 2867.3779.7863.71.1121.004[35]
S2-50100 × 2810.3751.7801.61.0781.001
S2-100100 × 2753.9731.1789.71.0310.955
S2-200100 × 2779.1692.9745.41.1241.045
S2-300100 × 2673.0668.6717.81.0070.938
S3-0100 × 3891.3818.3917.61.0890.971
S3-50100 × 3818.0736.0898.41.1110.911
S3-100100 × 3754.7787.2876.40.9590.861
S3-200100 × 3830.0739.2837.41.1230.991
S3-300100 × 3696.9691.1792.21.0080.880
S3.9-0100 × 3.91068.0840.01028.51.2711.038
S3.9-50100 × 3.91095.0940.51011.91.1641.082
S3.9-100100 × 3.91127.0950.01026.21.1861.098
S3.9-200100 × 3.91134.0938.3959.61.2091.182
S3.9-300100×3.91126.0956.3922.31.1771.221
Mean value1.1101.013
Standard deviation0.0070.011
SC30-T2.5-N080 × 2.5460.5 431.8 1.067[36]
SC30-T2.5-N6080 × 2.5468.7 431.2 1.087
SC30-T2.5-N8080 × 2.5458.2 430.9 1.063
SC30-T2.5-N10080 × 2.5420.4 430.7 0.976
Mean value 1.048
Standard deviation 0.002
Table 2. Bearing capacity comparisons between the numerical results and experimental results of specimens exposed to acid rain corrosion.
Table 2. Bearing capacity comparisons between the numerical results and experimental results of specimens exposed to acid rain corrosion.
Specimen IDB × t
(mm)
t
(mm)
γ
(%)
αNue
(kN)
Nce
(kN)
Nbe
(kN)
Nue/NceNue/Nbe
S-114-0114.00 × 2.970.000.00.113950.0912.0921.21.0421.031
S-114-1113.42 × 2.970.249.60.102970.0997.0985.00.9730.985
S-114-2112.78 × 2.970.5120.50.089950.0900.1902.51.0551.041
S-114-3112.20 × 2.970.7630.20.078850.0814.7846.31.0431.004
Mean value1.0281.018
Standard deviation0.0020.001
Table 3. Main design parameters of the models.
Table 3. Main design parameters of the models.
Model IDB × L × t
(mm)
t
(mm)
fcu
(Mpa)
fy
(Mpa)
γ
(%)
αNfnpN
(kN)
S-40-235-0.11-0400 × 1200 × 10040235100.1110008657
S-40-235-0.11-1400 × 1200 × 10140235100.1110017672
S-40-235-0.11-2400 × 1200 × 10240235100.1110026718
S-40-235-0.11-3400 × 1200 × 10340235100.1110035808
S-40-235-0.11-4400 × 1200 × 10440235100.1110045011
S-40-235-0.11-5400 × 1200 × 10540235100.1110054242
Note: S means that the section of the specimen is square. The first number represents the compressive strength of concrete cubes. The second number represents the yield strength of the steel tube. The third number represents the initial steel ratio of the specimens (α = As/Ac, where As and Ac denote the areas of the steel tube and concrete in the initial state, respectively). The fourth number represents the combined times of freeze–thaw cycles and acid rain corrosion. For example, S-40-235-0.11-4 specifies square CFST specimens, compressive strength of concrete of 40 MPa, yield strength of the steel tube of 235 MPa, initial steel ratio of 0.11, and four alterations.

Share and Cite

MDPI and ACS Style

Zhang, T.; Lyu, X.; Yu, Y. Prediction and Analysis of the Residual Capacity of Concrete-Filled Steel Tube Stub Columns under Axial Compression Subjected to Combined Freeze–Thaw Cycles and Acid Rain Corrosion. Materials 2019, 12, 3070. https://doi.org/10.3390/ma12193070

AMA Style

Zhang T, Lyu X, Yu Y. Prediction and Analysis of the Residual Capacity of Concrete-Filled Steel Tube Stub Columns under Axial Compression Subjected to Combined Freeze–Thaw Cycles and Acid Rain Corrosion. Materials. 2019; 12(19):3070. https://doi.org/10.3390/ma12193070

Chicago/Turabian Style

Zhang, Tong, Xuetao Lyu, and Yang Yu. 2019. "Prediction and Analysis of the Residual Capacity of Concrete-Filled Steel Tube Stub Columns under Axial Compression Subjected to Combined Freeze–Thaw Cycles and Acid Rain Corrosion" Materials 12, no. 19: 3070. https://doi.org/10.3390/ma12193070

APA Style

Zhang, T., Lyu, X., & Yu, Y. (2019). Prediction and Analysis of the Residual Capacity of Concrete-Filled Steel Tube Stub Columns under Axial Compression Subjected to Combined Freeze–Thaw Cycles and Acid Rain Corrosion. Materials, 12(19), 3070. https://doi.org/10.3390/ma12193070

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop