Next Article in Journal
Nano-Porous-Silicon Powder as an Environmental Friend
Next Article in Special Issue
Fused Filament Fabrication of NiTi Components and Hybridization with Laser Powder Bed Fusion for Filigree Structures
Previous Article in Journal
Comparison of the Toxicity of Pristine Graphene and Graphene Oxide, Using Four Biological Models
Previous Article in Special Issue
Sequential Processing of Cold Gas Sprayed Alloys by Milling and Deep Rolling
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Dual-Laser PBF-LB Processing of a High-Performance Maraging Tool Steel FeNiCoMoVTiAl

1
Rosswag GmbH, 76327 Pfinztal, Germany
2
Institute for Applied Materials-Materials Science and Engineering (IAM-WK), Karlsruhe Institute of Technology (KIT), 76131 Karlsruhe, Germany
3
wbk Institute of Production Science, Karlsruhe Institute of Technology (KIT), 76131 Karlsruhe, Germany
*
Author to whom correspondence should be addressed.
Materials 2021, 14(15), 4251; https://doi.org/10.3390/ma14154251
Submission received: 30 June 2021 / Revised: 23 July 2021 / Accepted: 27 July 2021 / Published: 29 July 2021
(This article belongs to the Special Issue Research and Development of Additive Manufacturing Technology)

Abstract

:
As part of an international research project (HiPTSLAM), the development and holistic processing of high-performance tool steels for AM is a promising topic regarding the acceptance of the laser powder bed fusion (PBF-LB) technology for functionally optimized die, forming and cutting tools. In a previous work, the newly developed maraging tool steel FeNiCoMoVTiAl was qualified to be processed by laser powder bed fusion (PBF-LB) with a material density of more than 99.9% using a suitable parameter set. To exploit further optimization potential, the influence of dual-laser processing strategies on the material structure and the resulting mechanical properties was investigated. After an initial calibration procedure, the build data were modified so that both lasers could be aligned to the same scanning track with a defined offset. A variation of the laser-based post-heating parameters enabled specific in-situ modifications of the thermal gradients compared to standard single-laser scanning strategies, leading to corresponding property changes in the produced material structure. An increase in microhardness of up to 15% was thus obtained from 411 HV up to 471 HV. The results of the investigation can be used to derive cross-material optimization potential to produce functionally graded high-performance components on PBF-LB systems with synchronized multi-laser technology.

1. Introduction

The industrial usage of metal additive manufacturing (AM) is steadily increasing in many branches and applications. For the tooling industry, the integration of internal channel structures enables new design possibilities with increased performance due to better heat transfer for die, forming and cutting applications [1,2,3]. The most common AM technology for high-quality metal parts is the laser powder bed fusion (PBF-LB) process [4]. The PBF-LB process enables functional benefits to the part with a higher freedom of design due to the layerwise manufacturing with metal powder as the starting material and a laser beam as the energy source for melting. The resulting material properties differ from conventional manufacturing routes due to the local micro-welding processes. The solidification after melting is characterized by high cooling rates (103–108 K/s) based on self-quenching by solidified previous layers and thus leading to fine-grained material microstructures [5,6].

1.1. High-Performance Tool Steels for PBF-LB

High-performance tool steels with emphasis on high hardness often contain high amounts of carbon (≥0.4 wt%), resulting in a poor weldability due to the increased hot cracking sensitivity. The PBF-LB processing of high-carbon steels with industrial standard PBF-LB systems and preheating temperatures of 200 °C or less thus often leads to cracking issues due to the high local stresses associated with the volumetric change during phase transformation as well as the repetitive heating and cooling cycles [7,8,9,10,11].
Maraging tool steels are high alloyed steels with more than 12 wt% nickel and known for their good mechanical properties, with a combination of high strength and toughness as well as high temperature strength, which leads to further potential for their function-optimized usage in the AM tooling industry [12]. Due to the low amount of carbon, with less than 0.03 wt%, the necessary weldability for PBF-LB processes is given. The optimization of the mechanical properties is based on the precipitation of intermetallic phases during aging in a common temperature range from 480 °C to 500 °C for 2 h to 6 h, which results in significantly higher hardness [13,14]. Furthermore, the possibility of short-term aging of maraging tool steels was demonstrated in a study by Marcisz and Stępień [15] for 18Ni350, leading to an increase in hardness from 340 HV to 600 HV with a temperature of 600 °C applied for only 15 s. The increased hardness was probably due to a redistribution of the atoms before precipitation.
For the additive manufacturing of mechanically loaded tools, the most common material in industrial PBF-LB systems is the maraging tool steel AISI 18Ni300. In the as-printed state, the alloy has an average hardness of around 330 HV, which leads to good machinability. The maximum hardness after heat treatment of 18Ni300 is limited in a range of around 540 HV to 665 HV [13,16,17]. Therefore, the resulting hardness is often not suitable for many applications in the tooling industry. Here, for example, high-speed steels such as the AISI M2 are broadly used with a hardness of more than 700 HV [13].
In a previous study, the newly developed maraging tool steel alloy FeNiCoMoVTiAl was initially qualified within a holistic process chain for use in standard PBF-LB systems [18]. The results showed good PBF-LB processability, with significantly higher hardness compared to the reference material 18Ni300 of nearly 700 HV after heat treatment.

1.2. Multi-Laser PBF-LB Processing

The industrial application of multi-laser PBF-LB scanning strategies started with the market readiness of the first commercially available multi-laser PBF-LB machines in 2011 [19]. The accompanying multi-laser scanning strategies were mainly based on stitching the scanning vectors of multiple lasers together in defined overlapping areas to build larger parts more efficiently and enable larger build spaces. The resulting influence of using multiple lasers to jointly build parts is exemplarily shown in [20].
Using multiple lasers on the same scanning track with a predefined offset is a field of research that is relatively underrepresented. There are some early but promising results from Abe et al. [21] that showed that the bending strength and hardness can be modified with a dual-laser scanning strategy through slower cooling or reheating. However, following studies mainly focused on the usage of a second laser beam for preheating the powder bed to reduce melting fumes [22] or to influence the density and surface quality with a very close following second laser beam [23]. Further findings in [24] based on simulations showed the possibility of reducing the thermal gradients by using a second defocused laser beam for post-heating. Other studies used multiple laser beams or laser diode area melting to obtain a higher build rate than the standard PBF-LB process based on the increased amount of energy sources applied simultaneously to the powder bed [25,26].
This paper focuses on the effects of a dual-laser processing strategy with the second laser beam used for in-situ heat treatment by remelting a fraction of the welded tracks with a delay of less than 10 ms. Part of the additional energy introduced by the subsequent laser track heats the surrounding material structure and modifies the thermal history. The resulting melt pool dimensions and hardness will be correlated with the varied process parameter sets to deepen the knowledge about the further application of dual-laser strategies. The presented results could furthermore be used to derive PBF-LB processing strategies for voxel-based graded material structures with maraging tool steels and other materials. Similar results based on modified thermal gradients were shown in [27] with directed energy deposition (DED) processes and a Fe19Ni5Ti steel designed for laser additive manufacturing leading to a Damascus-like metallic composite.

2. Experimental Setup

2.1. Material

The maraging tool steel FeNiCoMoVTiAl, also known under the trademark Specialis®, is based on a newly developed chemical composition, as shown in Table 1. The alloy is designed for good PBF-LB processability and higher hardness after heat treatment compared to other maraging steels. Other advantages of this alloy to be examined could be increased high-temperature strength and high-temperature hardness, which is an essential feature when using this alloy for applications in thermally stressed dies and tools.
The pre-alloyed material was atomized on a small batch atomizer AU 3000 system by BluePower Casting Systems GmbH (Walzbachtal, Germany). Further details about the system and the associated powder production process can be found in [28,29]. The resulting metal powder was processed according to PBF-LB powder specifications for good powder bed density and flowability. The analysis results regarding the particle size distribution, particle sphericity, flowability and residual moisture are shown in Table 2.

2.2. Machine

The experiments were conducted on the PBF-LB system SLM 280 1.0 Twin 400 W with gas flow upgrade by SLM Solutions Group AG (Lübeck, Germany). The optical system consisted of two water-cooled 400 W fiber lasers of 1070 nm wavelength (YLR-400-WC) by IPG Laser GmbH (Burbach, Germany), with each laser connected to an air-cooled and digitally controlled galvo system with varioSCAN by SCANLAB GmbH (Puchheim, Germany). The two laser systems were calibrated to work separately on their assigned half of the build plate and furthermore using stitching operations to produce larger parts within a predefined overlapping area of 280 mm × 30 mm (see Figure 1). A build volume reduction of 100 mm × 100 mm was used in this study to lower the amount of metal powder needed for a certain build height. To enable the synchronized switching and movement operations of both laser beams within the overlapping area, the two SCANLAB RTC®5 control cards were connected for synchronized clock rates in a master–slave mode. According to SCANLAB, a reproducible time lag of around 0.16 µs could be achieved [31]. While the standard machine control software (SLM MCS 2.3 Build 78) with a build processor exported file could not use the synchronization features, a special version of the MCS was provided by SLM Solutions Group AG. With this software update, the parameters for each scanning and jumping vector of the lasers could be defined individually by importing a specific formatted csv-table for a behavior analogous to G-code programming.

2.3. Double-Laser Exposure Strategy

The disadvantage of using the modified MCS with csv-file input lies in the inability to change the exposure strategy during the manufacturing process. The initially defined scanning and jumping vectors will be repeated within each layer and the common rotation of the scanning strategy for reducing the resulting material defects and thermally induced residual stresses cannot be implemented. Therefore, an exposure strategy was derived to enable a stable and reproducible manufacturing process to produce volumetric sample parts with two laser beams scanning the same vectors with a predefined offset. The exposure strategy is exemplarily shown in Figure 2. The offset between the two laser beams was regulated by a longer approach path for the start vector of one laser beam and remained constant during manufacturing due to the synchronized clock rates of the optical systems. Furthermore, an orientation angle of 45° regarding the recoater and gas flow direction was determined to eliminate negative impacts by recoating or melting parallel to the scanning vectors. With the shown exposure strategy, the resulting melting fumes of laser 1 should not lead to a negative influence of laser 2 as long as both laser beams are not working with an offset of one or multiple scanning vector lengths.

2.4. Calibration Procedure

Both optical systems and the associated controlling units of the two lasers must be calibrated to minimize the spatial and temporal deviations. For the spatial calibration, a simple pattern according to Figure 3 was created on multiple positions of a build plate within the reduced overlapping area of 100 mm × 30 mm. The possible deviations for X-axis and Y-axis were measured by microscopy. The optical systems were adjusted within the MCS so that all measured deviations were reproducibly smaller than 5 µm on both axes for a melt pool width of approximately 120 µm.
The temporal calibration was validated to some extent by creating the intersecting pattern according to Figure 4 on a build plate. Both laser beams were scanning along the respectively associated vectors, with one laser delayed at the start due to an extended vector. This delay will theoretically be compensated after scanning half of the vectors by a faster scanning speed. During analysis of the intersection points via microscopy, the subsequent laser beam could be identified by the overlying melt pool. The theoretical time lag of 0.16 µs was difficult to prove with this calibration approach because of the melting and solidification inertia consequently leading to merging melt pools if the two laser beams were intersecting in close succession. As a result, a reproducible time lag variation of 0.6 ms as a maximum could be derived regarding the used measurement approach. To determine this value, the vector length between the two intersection points with change in overlying melt pool was divided by the scanning velocity. We expected a significantly smaller variation in the time lag than the proven 0.6 ms because of the high reproducibility of measurement results during the test series.

2.5. Experimental Design

To investigate the influence of the dual-laser exposure strategies, a variation in post-heating parameters was used to produce volumetric samples for comparison with a standard single-laser and remelting strategy. In Figure 5, the main characteristics of the three production conditions regarding the energy input and resulting melting, solidification and in-situ heat treatment zones are shown. The elaborated dual-laser exposure strategies shown in Figure 5b were used to extend the time period of in-situ heat treatment compared to the single-laser processing in Figure 5a, with the goal of influencing the resulting mechanical properties of the maraging tool steel. If the offset distance between the two laser beams is substantially extended and the material has already a homogeneous temperature level when the second laser beam is approaching, an approximation of well-known remelting process conditions shown in Figure 5c should be obtained. Due to a less penetrating melt pool depth of the following laser beam in the dual-laser modes, the main approach is to eliminate the direct effects such as the melt pool boundaries of the remelted zones by the first laser during the following layer. Thus, a comparable material structure for all examined process conditions regarding the resulting melt pool patterns should be obtainable.
The parameter windows for single-laser exposure strategies are mainly described in the literature by laser power Plaser1, focal spot diameter dlaser1, scanning speed vscan, hatch distance dhatch and layer thickness dlayer. For expansion of these well-examined parameter windows, the second and following laser beam bring in additional degrees of freedom for adjusting the process conditions. As additional parameters in this study regarding the second laser beam, the laser power Plaser2, the focal spot diameter dlaser2 and the offset distance between the laser beams ∆offset were used.
Based on preliminary single-bead studies on FeNiCoMoVTiAl bulk material to derive optimized parameter sets for the PBF-LB processing, resulting melt pool dimensions for different process parameter sets were obtained. Due to the uniform exposure strategy, a sufficient overlapping of the melt pools for the first laser is necessary to reduce the occurrence probability of a lack of fusion defects according to Figure 6a. A good fitting parameter set was identified with Plaser1 of 200 W, dlaser1 of approximately 85 µm, vscan of 800 mm/s, dhatch of 0.85 mm and dlayer of 40 µm. The resulting melt pool based on the single-bead studies was characterized by a melt pool width W1 of around 85 µm and a melt pool depth D1 of around 120 µm. Furthermore, two different process parameters for the post-heating laser beam were identified to obtain a melt pool depth each of around 40 µm, which corresponded to the layer thickness. The first parameter set was defined with Plaser2 of 125 W and dlaser2 of around 85 µm, as shown in Figure 6b. The second dual-laser parameter set used the possibility to defocus the laser beam to dlaser2 of around 170 µm by the SCANLAB varioSCAN system to meet the melt pool depth limit of 40 µm despite an increased Plaser2 of 200 W, as shown in Figure 6c.
The summarized process parameter variations for the dual-laser parameter study are shown in Table 3. The influence of the subsequent laser beam will be investigated in an offset distance range from 1 mm to 4 mm. For ∆offset below 1 mm, strong negative effects on the process stability with delamination issues on the surface layer occurred during preliminary tests. A ∆offset of 2400 mm for DLR-125 and DLR-200 resulted from a 3 s time delay until the surface layer was remelted. In addition to the already defined process conditions, the dimensions of the volumetric test samples were specified to be 10 mm along the scanning vectors, 7 mm wide and around 8 mm high. The build plate preheating was turned off to exclude any influence by a potentially inhomogeneous heat distribution across the build plate surface. Furthermore, the time difference between the exposure processes of two successive layers was set to be 40 s, consisting of 30 s minimum exposure time and 10 s duration for powder recoating.

2.6. Evaluation Method

The plane for evaluation of the produced test samples was aligned, according to Figure 7, vertically to the scanning direction, with an offset of 2 mm to the as-build surface to eliminate edge effects. The cross-sections were ground, polished and analyzed regarding the material density three times in one layer by optical analysis with a Stemi 508 doc stereomicroscope by Carl Zeiss Industrielle Messtechnik GmbH (Oberkochen, Germany) and a 50× magnification. The area of the pores and cracks identified via a constant threshold of the gray value was related to the total area to determine the material density. For the measurements of the resulting melt pool dimensions in the top layer, the cross-sections were etched for 10–20 s with V2A etchant until the surface tarnished. Afterwards, the analysis was performed with the same microscope and a 500× magnification. The width and the depth of the melt pools for laser 1 and laser 2 were determined with 9 measurements each on different melt pools.
For microhardness testing within the melt pool centers from the surface layer downwards, a Q30A+ by ATM Qness GmbH (Mammelzen, Germany) was used. The Vickers hardness impressions were conducted for 10 s to maintain HV0.1 according to DIN EN ISO 6507-1:2018-07 [32]. For standard-compliant measurements, the distances between the roughly 65 hardness indentations were set to every second layer, which resulted in approximately 80 µm each.

3. Results and Discussion

3.1. Effect on Material Density

The measured material density values of the different process parameter sets are illustrated in Figure 8. The results show a good overall material density of more than 99.69% for all analyzed samples. In particular, the reference parameter sets SL, DLR-125 and DLR-200 shown in Figure 9a–c have a very high density of more than 99.92%, concluding stable process conditions for the sample manufacturing. There is even a slight material density improvement noticeable on a high level by remelting and thereby eliminating small accumulations on the weld tracks, which could lead to poorer powder deposition on the following layer. The material density determined for DL-125 is nearly constant on a high level of more than 99.89% for all examined offset distances. In comparison, the drop in the material density for DL-200 and ∆offset between 1 mm and 3 mm below 99.90% could be explained by more unstable process conditions due to the instant remelting process with a defocused 200 W powered laser beam. The second laser affects the topography of the surface layer by elevated weld tracks resulting from a higher temperature level and thus the following powder layer deposition as well as melting processes. Due to the layerwise repeated exposure strategies with identical scanning vectors, a buildup of unstable process conditions could occur. The resulting effect could be seen in Figure 9f, with noticeable surface-layer waviness and the tendency to have a higher porosity with larger voids for smaller ∆offset due to the higher amount of laser energy applied in the given time period. This explanation could be supported by the difference in material density between DL-125 with 99.90% and DL-200 with 99.70% for ∆offset of 1 mm. With 200 W laser power, the energy input is around 60% higher in just 1.25 ms after the melting process of the first laser. For ∆offset of 4 mm, also the DLR-200 shown in Figure 9g leads to a comparably high material density of 99.94% due to the longer cooling time between the two laser energy inputs.

3.2. Effect on Melt Pool Dimensions

For obtaining a better understanding of the melting and cooling behavior during the dual-laser PBF-LB processing, the resulting melt pool dimensions of the etched cross-sections were measured in the top layer. Width W1 and depth D1 of the melt pools are shown in Figure 10 for SL, DL-125 and DLR-125. For DL-200 and DLR-200, only D1 could be measured because of the overlapping melt pools of laser 2. As a reference for the melt pool dimensions of laser 1, the parameter set SL can be used. The measured values for D1 of 144 µm and W1 of 150 µm show a significant increase in the melt pool size compared to the preliminary single-bead studies. This increase could be explained by the higher temperature level of the part during the layerwise manufacturing process and therefore the lower energy input needed for reaching the melting temperature. While D1 is almost constant for all process parameter sets as expected, W1 shows some irregularities. The increased W1 for DL-125 and ∆offset of 4 mm could be explained by the approach of laser 1 to laser 2 on the previous scanning vector. Therefore, a higher temperature level on the surface is expected, which leads to an expansion of the upper region of the melt pool.
When it comes to the analysis of the melt pool dimensions for laser 2, shown in Figure 11, the influence of the defocused but higher-power parameter set DL-200 could be clearly seen in the increased W2 compared to DL-125, especially for ∆offset of 4 mm. For smaller ∆offset of 1 mm to 3 mm, W2 was more difficult to measure for DL-200 because of the already described surface-layer waviness resulting from more unstable process conditions. For DL-125, a slight trend could be obtained for a decreased W2 as ∆offset increases due to the longer cooling time between the laser energy inputs. In contrast to W2, the D2 values for DL-200 and DL-125 are nearly constant, resulting from a constant sub-surface temperature based on the laser 1 energy input and slower heat dissipation within the material.
When analyzing the etched cross-sections in Figure 12, only minor differences between the melt pool structures of the different parameter sets could be identified. Most of the resulting material structure was apparently only melted by laser 1 and only differed in the thermal history during the layerwise dual-laser PBF-LB processing. This shows a good implementation of the originally intended dual-laser exposure strategy, even though the resulting melt pool dimensions increased compared to the originally intended dimensions due to the higher energy input and associated temperature level of the part during PBF-LB processing.

3.3. Effect on Micro Hardness

In Figure 13, an exemplary hardness profile is shown for SL, which is typical for all evaluated hardness results. A significant drop in the hardness within an area of around 400 µm below the surface layer could be seen for all samples until the hardness values ranged around a stable hardness level of 441 HV. The reason for this drop could be seen in the process-related temperature history and the need for multiple heating and cooling cycles on a higher temperature level for receiving the respective hardness. In order not to influence the following evaluations too strongly by the effect near the surface, only measured values below the 400 µm distance are considered.
The mean values and standard deviations for the microhardness examination of the different process parameter sets and offsets are shown in Figure 14. The hardness level of SL, with around 441 HV0.1, can be seen as a reference value for the evaluation of the dual-laser and remelting parameter sets. For the dual-laser processing with offset distances between 1 mm and 4 mm, the results show a significant trend to a higher microhardness, with values up to 471 HV0.1 for DL-125 and DL-200. Although DL-125 sets the overall maximum hardness with ∆offset of 1 mm, the DL-200 parameters show a more constant hardness level between 462 HV and 470 HV. Due to the microhardness testing, the slightly lower porosity of the DL-200 parameter sets below ∆offset of 4 mm has no detectable influence on the hardness. For ∆offset from 1.5 mm to 4 mm, the hardness level for DL-125 drops down to a minimum value of 440 HV, with an almost continuous progression. The assumption is thus that the energy input for DL-125 is only sufficient to trigger the significant hardness increase effects such as short-term aging in the material for very short ∆offset values below approximately 1.5 mm. In the case of DL-200, this more stable hardness increase effect can be explained by the higher energy input and the associated longer holding time at a higher temperature level in the in-situ heat treatment zone. Due to the slower heat dissipation processes below the surface, the DL-200 parameter sets appear to be more independent of variation of ∆offset. The examination of the remelting parameter sets shows DLR-200 at a comparable hardness level with SL. For DLR-125, the hardness significantly decreases below the hardness of SL to around 411 HV0.1. Obviously, there is a material-specific effect discovered for ∆offset between 4 mm and 2400 mm that leads to a decreased hardness. Possibly, a solution annealing process is started due to the time-delayed reheating of the in-situ heat treatment zones leading to this effect.
All these detected changes in hardness levels for the different process conditions could be related to material-specific effects based on the different temperature histories during the manufacturing process. Shorter distances and higher energy inputs of the subsequent laser beam lead to harder materials and remelting parameters lead to softer material properties compared to standard single-laser process parameters.

3.4. Observed Potential for Functionally Graded Materials by Double-Laser PBF-LB Processing

To reach the full potential of voxel-based manufacturing in PBF-LB, applicable processing strategies and suitable materials must be qualified. The needed PBF-LB systems for using multiple laser beams at least in a certain overlapping area are already commercially available and the further strategy of the system OEMs already tends towards larger systems with more lasers. The identified changes in hardness related to different process parameter sets and the resulting thermal histories could be used for an intentionally graded modification in the mechanical properties of additively manufactured parts. Due to the consistent melt pool structure for all considered parameter sets, no negative effects are assumed if the parameter sets are changed on certain regions during part production. This could be one of the main advantages for the specific adjustment of the in-situ heat treatment parameters with a subsequent laser beam compared to modified single-laser parameters with significant changes in melt pool geometries during part manufacturing. In particular, when using a material for tooling applications, such as the newly developed maraging FeNiCoMoVTiAl alloy, a functionally graded material structure could be used to produce parts with hard and wear-resistant outer surfaces in conjunction with ductile core regions. As the hardness changes are derived from material-specific effects due to the different thermal histories while processing, there is furthermore a chance of maintaining these graded properties even through a subsequent aging heat treatment process of the part. However, a further solution heat treatment will eliminate the discovered hardness changes by dissolving the characteristic PBF-LB microstructure.

4. Conclusions

The results show the feasibility of dual-laser PBF-LB processing of the maraging tool steel FeNiCoMoVTiAl by using a second laser beam for post-heating and remelting a fraction of the previously welded tracks for the modification of in-situ heat treatment conditions. A sufficient calibration procedure and minor hardware modifications are needed to build volumetric parts with a uniform exposure strategy based on a G-code-like vector dataset. Furthermore, the main results for the different evaluation methods are listed below:
  • A material density of more than 99.69% was obtained for all tested parameter sets. The best density results were determined for single-laser and remelting parameters with more than 99.92%. The dual-laser parameters with the subsequent 125 W laser beam resulted in a material density of more than 99.89% due to the more stable processing conditions in comparison to the dual-laser parameters with 200 W.
  • Significant changes in the resulting melt pool dimensions regarding the parameter variations of the subsequent laser beam were measured on the surface layer. As a result of the elaborated exposure strategies, a consistent melt pool structure was still obtainable for all tested parameter sets.
  • The modified dual-laser process parameter sets led to a significant hardness change compared to single-laser PBF-LB processing with around 441 HV0.1. An increase by around 30 HV0.1 was obtained by using the dual-laser exposure strategies. A higher laser power as well as a shorter offset distance of the subsequent laser beam appear to have hardness-increasing effects on the resulting material structure. Possibly, short-time aging effects of the in-situ heat treatment zone could be the reason for the hardness increase. A hardness decrease by around 30 HV0.1 compared to the single laser parameter was determined by a remelting strategy with 125 W laser power. Solution annealing effects within the heat-affected zone could be a possible explanation for this.
  • The adjustable hardness levels for the different dual-laser parameter sets in combination with no significant changes in the resulting melt pool structure open new possibilities to produce functionally graded material structures by dual-laser PBF-LB processing.
Further research will be conducted regarding the necessary heat treatment after dual-laser PBF-LB processing to receive the material-specific properties of maraging tool steels. Ideally, a heat treatment process can be identified that also preserves the functionally graded effects when several processing conditions are combined in one component. This would enable the pursuit of industrial application of the results.

Author Contributions

Conceptualization, investigation, methodology, project administration and writing—original draft preparation, G.G.; data curation and validation, G.G. and N.N.; writing—review and editing, N.N., S.D., F.Z. and V.S.; supervision, S.D., F.Z. and V.S. All authors have read and agreed to the published version of the manuscript.

Funding

The research project “Design of high-performance tool steel metal powders for Laser Additive Manufacturing (HiPTSLAM)” is funded by the Federal Ministry of Education and Research (BMBF) in the program “Internationalisation of Leading-Edge Clusters, Forward-Looking Projects and Comparable Networks (InterSpiN)” under the funding code 03INT614B and supervised by Project Management Jülich (PTJ).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The data presented in this study are available on request from the corresponding author after obtaining permission of authorized person.

Acknowledgments

The authors thank the German HiPTSLAM project partners Blue Power Casting Systems and Gühring for their cooperation prior to this work. Special thanks go to Jörg Fischer-Bühner and Tobias Müller. Kaj Berggreen from SLM Solutions deserves special thanks for aiding in the necessary system modification and therefore making the implementation of the dual-laser PBF-LB processing possible.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Santhoshsarang, D.M.; Divya, K.; Telasang, G.; Soundarapandian, S.; Bathe, R.; Padmanabham, G. Additively manufactured high-performance conformally cooled H13 tool steel die insert for pressure die casting. Trans. Indian Natl. Acad. Eng. 2021, 1–12. [Google Scholar] [CrossRef]
  2. Chantzis, D.; Liu, X.; Politis, D.J.; El Fakir, O.; Chua, T.Y.; Shi, Z.; Wang, L. Review on additive manufacturing of tooling for hot stamping. Int. J. Adv. Manuf. Technol. 2020, 109, 87–107. [Google Scholar] [CrossRef]
  3. Shinde, M.S.; Ashtankar, K.M. Additive manufacturing–assisted conformal cooling channels in mold manufacturing processes. Adv. Mech. Eng. 2017, 9, 1687814017699764. [Google Scholar] [CrossRef]
  4. Munsch, M.; Schmidt-Lehr, M.; Wycisk, E. AMPOWER Report: Metal Additive Manufacturing. 2020. Available online: https://additive-manufacturing-report.com/ (accessed on 25 June 2021).
  5. Herzog, D.; Seyda, V.; Wycisk, E.; Emmelmann, C. Additive manufacturing of metals. Acta Mater. 2016, 117, 371–392. [Google Scholar] [CrossRef]
  6. Meier, C.; Penny, R.W.; Zou, Y.; Gibbs, J.S.; Hart, A.J. Thermophysical phenomena in metal additive manufacturing by selective laser melting: Fundamentals, modeling, simulation and experimentation. Annu. Rev. Heat Transfer. 2017, 20, 241–316. [Google Scholar] [CrossRef]
  7. Wu, L.; Das, S.; Gridin, W.; Leuders, S.; Kahlert, M.; Vollmer, M.; Niendorf, T. Hot work tool steel processed by laser powder bed fusion: A review on most relevant influencing factors. Adv. Eng. Mater. 2021, 23, 2100049. [Google Scholar] [CrossRef]
  8. Saewe, J.; Carstensen, N.; Kürnsteiner, P.; Jägle, E.A.; Schleifenbaum, J.H. Influence of increased carbon content on the processability of high-speed steel HS6-5-3-8 by laser powder bed fusion. Addit. Manuf. 2021, 46, 102125. [Google Scholar] [CrossRef]
  9. Bajaj, P.; Hariharan, A.; Kini, A.; Kürnsteiner, P.; Raabe, D.; Jägle, E.A. Steels in additive manufacturing: A review of their microstructure and properties. Mater. Sci. Eng. A 2020, 772, 138633. [Google Scholar] [CrossRef]
  10. Casati, R.; Lemke, J.N.; Tuissi, A.; Vedani, M. Aging behaviour and mechanical performance of 18-Ni 300 steel processed by selective laser melting. Metals 2016, 6, 218. [Google Scholar] [CrossRef]
  11. Casati, R.; Coduri, M.; Lecis, N.; Andrianopoli, C.; Vedani, M. Microstructure and mechanical behavior of hot-work tool steels processed by selective laser melting. Mater. Charact. 2018, 137, 50–57. [Google Scholar] [CrossRef]
  12. Turk, C.; Zunko, H.; Aumayr, C.; Leitner, H.; Kapp, M. Advances in maraging steels for additive manufacturing. Berg. Huettenmaenn Mon. 2019, 164, 112–116. [Google Scholar] [CrossRef] [Green Version]
  13. Song, J.; Tang, Q.; Feng, Q.; Ma, S.; Setchi, R.; Liu, Y.; Han, Q.; Fan, X.; Zhang, M. Effect of heat treatment on microstructure and mechanical behaviours of 18Ni-300 maraging steel manufactured by selective laser melting. Opt. Laser Technol. 2019, 120, 105725. [Google Scholar] [CrossRef]
  14. Jägle, E.A.; Choi, P.-P.; Van Humbeeck, J.; Raabe, D. Precipitation and austenite reversion behavior of a maraging steel produced by selective laser melting. J. Mater. Res. 2014, 29, 2072–2079. [Google Scholar] [CrossRef] [Green Version]
  15. Marcisz, J.; Stępień, J. Short-time ageing of MS350 maraging steel with and without plastic deformation. Arch. Metall. Mater. 2014, 59, 513–520. [Google Scholar] [CrossRef]
  16. Bai, Y.; Wang, D.; Yang, Y.; Wang, H. Effect of heat treatment on the microstructure and mechanical properties of maraging steel by selective laser melting. Mater. Sci. Eng. A 2019, 760, 105–117. [Google Scholar] [CrossRef]
  17. Kučerová, L.; Zetková, I.; Jandová, A.; Bystrianský, M. Microstructural characterisation and in-situ straining of additive-manufactured X3NiCoMoTi 18-9-5 maraging steel. Mater. Sci. Eng. A 2019, 750, 70–80. [Google Scholar] [CrossRef]
  18. Graf, G.; Neuenfeldt, M.; Müller, T.; Fischer-Bühner, J.; Beckers, D.; Donisi, S.; Zanger, F.; Schulze, V. Efficient qualification strategy of new steel alloys for laser powder bed fusion. Adv. Mater. Res. 2021, 1161, 27–36. [Google Scholar] [CrossRef]
  19. SLM Solutions Group, A.G. Eigenkapitalforum. 2019. Available online: https://www.slm-solutions.com/fileadmin/Content/Investor_Relations/29_SLM__Eigenkapitalforum_20191126.pdf (accessed on 25 June 2021).
  20. Masoomi, M.; Thompson, S.M.; Shamsaei, N. Quality part production via multi-laser additive manufacturing. Manuf. Lett. 2017, 13, 15–20. [Google Scholar] [CrossRef]
  21. Abe, F.; Osakada, K.; Shiomi, M.; Uematsu, K.; Matsumoto, M. The manufacturing of hard tools from metallic powders by selective laser melting. J. Mater. Process. Technol. 2001, 111, 210–213. [Google Scholar] [CrossRef]
  22. Heeling, T.; Gerstgrasser, M.; Wegener, K. Investigation of Selective Laser Melting Spatter Characteristics for Single- and Multi-Beam Strategies Using High Speed Imaging. 2017. Available online: https://www.wlt.de/lim/Proceedings2017/Data/PDF/Contribution10_final.pdf (accessed on 25 June 2021).
  23. Heeling, T.; Wegener, K. The effect of multi-beam strategies on selective laser melting of stainless steel 316L. Addit. Manuf. 2018, 22, 334–342. [Google Scholar] [CrossRef]
  24. Heeling, T.; Wegener, K. Computational investigation of synchronized multibeam strategies for the selective laser melting process. Phys. Procedia 2016, 83, 899–908. [Google Scholar] [CrossRef] [Green Version]
  25. Zavala-Arredondo, M.; Boone, N.; Willmott, J.; Childs, D.T.; Ivanov, P.; Groom, K.; Mumtaz, K. Laser diode area melting for high speed additive manufacturing of metallic components. Mater. Des. 2017, 117, 305–315. [Google Scholar] [CrossRef]
  26. Tsai, C.-Y.; Cheng, C.-W.; Lee, A.-C.; Tsai, M.-C. Synchronized multi-spot scanning strategies for the laser powder bed fusion process. Addit. Manuf. 2019, 27, 1–7. [Google Scholar] [CrossRef]
  27. Kürnsteiner, P.; Wilms, M.B.; Weisheit, A.; Gault, B.; Jägle, E.A.; Raabe, D. High-strength damascus steel by additive manufacturing. Nature 2020, 582, 515–519. [Google Scholar] [CrossRef] [PubMed]
  28. Schwenck, D.; Ellendt, N.; Fischer-Bühner, J.; Hofmann, P.; Uhlenwinkel, V. A novel convergent–divergent annular nozzle design for close-coupled atomisation. Powder Metall. 2017, 60, 198–207. [Google Scholar] [CrossRef]
  29. Schwenck, D.; Ellendt, N.; Mädler, L.; Fischer-Bühner, J.; Hofmann, P.; Uhlenwinkel, V. Generation of small batch high quality metal powder. Powder Metall. 2014, 57, 171–175. [Google Scholar] [CrossRef]
  30. DIN EN ISO 4490:2018-08. Metallpulver—Bestimmung der Durchflussrate mit Hilfe eines kalibrierten Trichters (Hall Flowmeter) (ISO_4490:2018); Deutsche Fassung EN_ISO_4490: Berlin, Germany, 2018. [Google Scholar]
  31. SCANLAB, Installation und Inbetriebnahme RTC®5 PCI-Karte, RTC®5 PCI-Express-Karte, RTC®5 PC/104-Plus-Karte und RTC®5 PCIe/104-Karte für die Scan-Kopf- und Lasersteuerung in Echtzeit. 2015. Available online: https://www.manualslib.de/manual/351204/Scanlab-Rtc-5.html (accessed on 25 June 2021).
  32. DIN EN ISO 6507-1:2018-07. Metallische Werkstoffe—Härteprüfung nach Vickers—Teil_1: Prüfverfahren (ISO_6507-1:2018); Deutsche Fassung EN_ISO_6507-1: Berlin, Germany, 2018. [Google Scholar]
Figure 1. Illustration of the PBF-LB system configuration to achieve dual-laser processing.
Figure 1. Illustration of the PBF-LB system configuration to achieve dual-laser processing.
Materials 14 04251 g001
Figure 2. Dual-laser scanning strategy for specimen manufacturing.
Figure 2. Dual-laser scanning strategy for specimen manufacturing.
Materials 14 04251 g002
Figure 3. Illustration of the procedure for spatial calibration.
Figure 3. Illustration of the procedure for spatial calibration.
Materials 14 04251 g003
Figure 4. Illustration of procedure for temporal calibration.
Figure 4. Illustration of procedure for temporal calibration.
Materials 14 04251 g004
Figure 5. Longitudinal section of the PBF-LB processing with (a) single laser, (b) dual-laser in-situ heat treatment and (c) dual-laser remelting strategy.
Figure 5. Longitudinal section of the PBF-LB processing with (a) single laser, (b) dual-laser in-situ heat treatment and (c) dual-laser remelting strategy.
Materials 14 04251 g005
Figure 6. Expected structure with resulting width and depth of the melt pools related to laser 1 (W1 and D1) and to laser 2 (W2 and D2) for (a) single-laser, (b) dual-laser with Plaser2 of 125 W and dlaser2 of around 85 µm and (c) dual-laser with Plaser2 of 200 W and dlaser2 of around 170 µm.
Figure 6. Expected structure with resulting width and depth of the melt pools related to laser 1 (W1 and D1) and to laser 2 (W2 and D2) for (a) single-laser, (b) dual-laser with Plaser2 of 125 W and dlaser2 of around 85 µm and (c) dual-laser with Plaser2 of 200 W and dlaser2 of around 170 µm.
Materials 14 04251 g006
Figure 7. Illustration of resulting cubic test specimen and the preparation plane for further examinations of material density, melt pool structure and hardness.
Figure 7. Illustration of resulting cubic test specimen and the preparation plane for further examinations of material density, melt pool structure and hardness.
Materials 14 04251 g007
Figure 8. Measured material density values of the samples produced using the listed parameters.
Figure 8. Measured material density values of the samples produced using the listed parameters.
Materials 14 04251 g008
Figure 9. Resulting cross-sections for material density measurements of the parameter sets (a) SL, (b) DLR-125, (c) DLR-200, (d) DL-125 with ∆offset of 1 mm, (e) DL-125 with ∆offset of 4 mm (f) DL-200 with ∆offset of 1 mm and (g) DL-200 with ∆offset of 4 mm.
Figure 9. Resulting cross-sections for material density measurements of the parameter sets (a) SL, (b) DLR-125, (c) DLR-200, (d) DL-125 with ∆offset of 1 mm, (e) DL-125 with ∆offset of 4 mm (f) DL-200 with ∆offset of 1 mm and (g) DL-200 with ∆offset of 4 mm.
Materials 14 04251 g009
Figure 10. Measured melt pool dimensions ((a) width W1 and (b) depth D1) in top layer resulting from laser 1 for the examined process parameter sets.
Figure 10. Measured melt pool dimensions ((a) width W1 and (b) depth D1) in top layer resulting from laser 1 for the examined process parameter sets.
Materials 14 04251 g010
Figure 11. Measured melt pool dimensions ((a) width W2 and (b) depth D2) in top layer resulting from laser 2 for the examined process parameter sets.
Figure 11. Measured melt pool dimensions ((a) width W2 and (b) depth D2) in top layer resulting from laser 2 for the examined process parameter sets.
Materials 14 04251 g011
Figure 12. Melt pool cross-sections for measurements of the melt pool dimensions and material structure analysis of the parameter sets (a) SL, (b) DLR-125, (c) DLR-200, (d) DL-125 with ∆offset of 1 mm, (e) DL-125 with ∆offset of 4 mm (f) DL-200 with ∆offset of 1 mm and (g) DL-200 with ∆offset of 4 mm.
Figure 12. Melt pool cross-sections for measurements of the melt pool dimensions and material structure analysis of the parameter sets (a) SL, (b) DLR-125, (c) DLR-200, (d) DL-125 with ∆offset of 1 mm, (e) DL-125 with ∆offset of 4 mm (f) DL-200 with ∆offset of 1 mm and (g) DL-200 with ∆offset of 4 mm.
Materials 14 04251 g012
Figure 13. Exemplary microhardness profile over build height of the parameter set SL.
Figure 13. Exemplary microhardness profile over build height of the parameter set SL.
Materials 14 04251 g013
Figure 14. Measured microhardness values of the samples produced with the different process parameter sets.
Figure 14. Measured microhardness values of the samples produced with the different process parameter sets.
Materials 14 04251 g014
Table 1. Chemical composition of the maraging tool steel Specialis®.
Table 1. Chemical composition of the maraging tool steel Specialis®.
ElementFeCNiCoMoTiVAl
wt%Bal.0.0218.3311.394.44<2<2<0.5
Table 2. Powder specification according to VDI 3405 Blatt 2:2013-08.
Table 2. Powder specification according to VDI 3405 Blatt 2:2013-08.
Powder Parameter ValuesMeasurement Method
Particle size distributiond10,3 (µm)19.32Dynamic particle imaging with Camsizer X2 by Retsch GmbH (Haan, Germany)
d50,3 (µm)32.30
d90,3 (µm)54.91
Particle sphericitySPHT30.85
Flowability(s/50 g)14.86Hall flowmeter according to DIN EN ISO 4490:2018 [30]
Residual moisture(%)<5humimeter RH2 by Schaller Messtechnik GmbH (St. Ruprecht an der Raab, Austria)
Table 3. Overview of parameter sets for the specimen manufacturing.
Table 3. Overview of parameter sets for the specimen manufacturing.
Parameter SetAcronymPlaser2 (W)dlaser2 (µm)offset (mm)
Reference single-laserSL0--
Double-laser 125 WDL-125125851, 1.5, 2, 2.5, 3, 4
Reference remelting 125 WDLR-125125852400
Double-laser 200 WDL-2002001701, 1.5, 2, 2.5, 3, 4
Reference remelting 200 WDLR-2002001702400
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Graf, G.; Nouri, N.; Dietrich, S.; Zanger, F.; Schulze, V. Dual-Laser PBF-LB Processing of a High-Performance Maraging Tool Steel FeNiCoMoVTiAl. Materials 2021, 14, 4251. https://doi.org/10.3390/ma14154251

AMA Style

Graf G, Nouri N, Dietrich S, Zanger F, Schulze V. Dual-Laser PBF-LB Processing of a High-Performance Maraging Tool Steel FeNiCoMoVTiAl. Materials. 2021; 14(15):4251. https://doi.org/10.3390/ma14154251

Chicago/Turabian Style

Graf, Gregor, Niki Nouri, Stefan Dietrich, Frederik Zanger, and Volker Schulze. 2021. "Dual-Laser PBF-LB Processing of a High-Performance Maraging Tool Steel FeNiCoMoVTiAl" Materials 14, no. 15: 4251. https://doi.org/10.3390/ma14154251

APA Style

Graf, G., Nouri, N., Dietrich, S., Zanger, F., & Schulze, V. (2021). Dual-Laser PBF-LB Processing of a High-Performance Maraging Tool Steel FeNiCoMoVTiAl. Materials, 14(15), 4251. https://doi.org/10.3390/ma14154251

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop