Next Article in Journal
Computation of High-Performance Concrete Compressive Strength Using Standalone and Ensembled Machine Learning Techniques
Next Article in Special Issue
Tribological Behavior and Microstructural Analysis of Atmospheric Plasma Spray Deposited Thin Coatings on Cardan Cross Spindles
Previous Article in Journal
Additives Imparting Antimicrobial Properties to Acrylic Bone Cements
Previous Article in Special Issue
Structural Response of Bonded Joints between FRP Composite Strips and Steel Plates
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Diagonal Tensile Test on Masonry Panels Strengthened with Textile-Reinforced Mortar

by
Dragoș Ungureanu
1,*,
Nicolae Țăranu
1,2,
Dan Alexandru Ghiga
1,
Dorina Nicolina Isopescu
1,
Petru Mihai
1 and
Ruxandra Cozmanciuc
1
1
Faculty of Civil Engineering and Building Services, “Gheorghe Asachi” Technical University of Iaşi, 43 Mangeron Blvd., 700050 Iaşi, Romania
2
The Academy of Romanian Scientists, 54 Splaiul Independentei, Sector 5, 050094 Bucuresti, Romania
*
Author to whom correspondence should be addressed.
Materials 2021, 14(22), 7021; https://doi.org/10.3390/ma14227021
Submission received: 30 September 2021 / Revised: 12 November 2021 / Accepted: 14 November 2021 / Published: 19 November 2021
(This article belongs to the Special Issue Advanced Materials for Multifunctional Applications)

Abstract

:
This study presents the results of an experimental and numerical program carried out on unreinforced masonry panels strengthened by textile-reinforced mortar (TRM) plastering. For this purpose, five panels were constructed, instrumented and tested in diagonal shear mode. Two panels were tested as reference. The first reference panel was left unstrengthened, while the second one was strengthened by a traditional self-supporting cement mortar matrix reinforced with steel meshes. The remaining three panels were strengthened by TRM plastering applied on one or both faces and connected with transversal composite anchors. The numerical and the experimental results evidenced a good effectiveness of the TRM systems, especially when applied on both panel facings.

1. Introduction

Unreinforced masonry (URM) has a long history of being the predominant building technique in Romania and in Europe. A large share of this existing building stock consists of historical monuments, which have been designed to resist only gravitational loads or, in many cases, have not been designed at all, but simply erected according to a few generic rules of common practice [1,2,3,4,5,6,7]. In Romania, the regions where the masonry monumental buildings lie are all characterized by medium-to-high levels of seismic hazard. The composite nature of the bricks and of the mortar, the stocky arrangement of the URM walls and the almost zero tensile capability of the masonry material makes this structural system potentially vulnerable to seismic actions [8,9,10,11,12]. Consequently, most of the existing URM buildings require strengthening interventions works, to adapt the capabilities of the structural system to the requirements of the current seismic design codes. In order to design and perform a particular strengthening technique, the structural behavior and the possible failure modes of the unstrengthened structure should be well analyzed.
During seismic excitation, URM structures can develop two possible types of dominant failure modes, the in-plane shear or the out-of-plane bending mechanisms [13,14]. The second mechanism can be avoided by improving the overall stiffness of the structure with additional transversal connections [15]. On the other hand, the in-plane shear capacity governs the global seismic performances of the URM structures, since the lateral loads from the load bearing walls are transferred through the in-plane path to the foundations [16]. The in-plane dominant failure mechanism can be divided in several characteristic modes, including failure by sliding, rocking, toe crushing and shear. Due to the high weight of the URM buildings, the in-plane failure by sliding is rarely developed. The in-plane rocking and toe crushing failures are the most ductile ones. Nonetheless, the in-plane shear is a brittle and sudden-failure mechanism, being more severe and dangerous than the other in-plane modes. Moreover, the shear failure mode can be developed during moderate or even small earthquakes and its level of severity is influenced by a large variety of parameters, including bricks and mortar quality, load bearing walls thickness and arrangement, age of the structure, type of materials, existing seismic protection, soil conditions and modal characteristics of the URM structure. For these reasons, the development and improvement of shear strengthening techniques for URM structures have been topics of interest for many researchers.
Originally, the reinforced concrete strengthening techniques were adopted for URM elements as well [17]. These traditional strengthening techniques consist in stitching or filling the cracks and plastering the masonry element with a self-supporting cement mortar matrix reinforced with steel meshes. The main disadvantage of this approach consists in the high additional weight provided by the steel reinforcements. In order to overcome this issue, various fiber-reinforced polymer (FRP) composite elements have been developed as an alternative to steel reinforcements. Despite their advantageous features, such as high strength-to-weight ratio and ease of application [18,19,20], using FRP composite elements in strengthening applications for URM structures is usually associated with several possible limitations. These are the potential debonding of externally applied FRP strips, the incompatibility between most of the epoxy systems and many types of substrates (due to the large stiffness discrepancies) and the unsatisfactory behavior of common resin products at high and low temperatures. Recently, besides the conventional FRP composite strengthening systems, new materials have been developed and exploited for URM structures’ retrofitting. Among these materials, the textile-reinforced mortar (TRM) is considered to be highly beneficial since it has an improved compatibility with masonry substrates. This strengthening system consists in a layer of an inorganic matrix (usually a cement-based mortar) that is reinforced and applied on one or both faces of the URM walls. The reinforcements are textile fabric meshes made of fiber roving ply arranged on at least two orthogonal directions. The mechanical properties of the textile reinforcements are controlled by the amount of roving and their orientation, while the level of penetration of the mortar matrix is influenced by the mesh spacings [5,21].
According to previous studies [1,22,23,24,25,26,27], the TRM strengthening systems designed for URM structures are promising solutions that can provide significant increments in terms of shear capacity and pseudo-ductility both for in-plane and out-of-plane loading conditions. The in-plane structural behavior of the URM strengthened with TRM was studied for various wall types and configurations, including one-leaf or two-leaf brick arrangements [28,29,30,31] and tuff volcanic masonry walls [32,33]. The outcomes of some of the most relevant experimental programs related to the shear capabilities of URM walls strengthened with TRM are summarized in Table 1 [34]. The test types are abbreviated as follows: DG—diagonal test; CY—cycling test; SH—shear test. BR and VT stand for brick and volcanic tuff masonries, while the fiber meshes are denoted with S for steel, G for glass, C for carbon and B for basalt. The strength and the deformation ratios represent the capacities of the strengthened masonry specimens reported to the capacities of the URM ones.
By studying the data presented in Table 1, it can be observed that, for all the experimental campaigns, the improved behavior of the URM panels strengthened with TRM, in terms of strength and deformation capacity, has been validated. However, in some cases, the effective amount of reinforcement was not sufficient to provide significant increases in strength, but it enhanced efficiently the displacement capacity. The latter was proved to be valid even for TRM systems which consists of flax fabrics. In addition, when used as a component of TRM systems, these types of fibers do not evidence severe degradation of their mechanical properties even if they are subjected to various environmental exposures and aging protocols [35,36].
The experimental campaigns cited in Table 1 were aimed to characterize the structural behavior of the TRM systems either by testing samples made from fibers and mortar (tensile and adherence tests) or by addressing the global characterization of the systems by means of diagonal compression tests on reinforced masonry panels. By comparing these types of experimental results with the ones obtained by applying the available theoretical models, other studies reported several limitations of the theoretical models, related to the inability to consider combined or non-standard failure modes [43].
Moreover, despite the available studies carried out to investigate the shear structural behavior of the URM strengthened with TRM, which highlighted the effectiveness of this type of strengthening system, some important aspects have still not been fully investigated. The latter may refer to anchorage methods for masonry walls which enable intervention works on both faces (the side-to-side connection) or on a singular face (the middle-to-side connection); the increase in lateral capacity based on the type and configuration of the transversal connectors, pattern and effective length for various types of anchorages; the characteristic failure modes for the systems with additional reinforcement due to the radial ends of the anchorages; and the synchronization between the experimental and numerical analyses based on adapted modelling strategies.
This paper reports the results obtained through a numerical and experimental program that was carried out at the Laboratory of Heavy Structure, located at the Faculty of Civil Engineering and Building Services in Iași. The masonry materials and the strengthening systems, both traditional and modern, are rather common in Romania. In particular, five URM panels were constructed, instrumented and tested in diagonal shear mode. In addition, all the specimens were micro-modelled and subjected to a nonlinear finite element analysis using the Ansys Workbench software. Two panels were tested as reference. The first reference panel was left unstrengthened, while the second one was strengthened through a traditional self-supporting cement mortar matrix reinforced with steel meshes. The remaining three panels were strengthened by TRM plastering applied on one or both faces and connected with transversal composite anchors. After a detailed experimental set-up and testing procedures, the main experimental results and the key features of each configuration of the strengthening system are reported. In addition, the experimental results are compared to the ones obtained through a micro-detailed finite element analysis and a general good agreement is found.

2. Experimental Set-Up

2.1. URM Panel Specimens’ Configurations and Materials Properties

The experimental program was performed on five 1200 × 1200 × 115 mm URM panels. The specimens were manufactured using brick clay masonry units (Figure 1) and normal mortar of M15 class [44]. All of the URM panels were constructed by qualified masons to insure a proper level of craftmanship, similar to current practice. The general configuration of the specimens is presented in Figure 2.
The URM panels were left to cure for 28 days. Prior to strengthening and testing, the mechanical characteristics of the masonry material were determined and compared to the ones provided by the manufacturer. Bricks were the first component of the URM panels to be investigated.
Tests to determine the compressive strength were performed on five real-size specimens (Figure 3), which were loaded in compression in a Zwick Roell 1000kN universal testing machine, according to the specifications given in the Norm SR EN 772-1+A1 [45]. The value of the compressive strength provided by the manufacturer (15 MPa) was 28% lower compared to the average value that was determined experimentally (20.83 MPa). The computed standard deviation (σ = 0.45) indicates that the values tend to be close to the mean. Thus, it can be concluded that the experimentally determined values of the compressive strength of the brick units showed no statistically significant differences.
The aim of the micro, non-linear analysis that is presented in Section 3 of this work is to provide a numerical model for designing purposes. Thus, the compressive strength provided by the manufacturer (the conservative value) was adopted.
Flexural and compression tests were performed to evaluate mortar strength, according to EN 1015-11 [46] (Figure 4). The flexural tests were made on a mortar prism (mortar type S) with the nominal dimensions of 40 × 40 × 160 mm, which were subjected to three-point bending loading. Each of the two parts of the mortar prisms that resulted from the flexural tests were used for the compression tests. A total number of 15 mortar prisms were subjected to the flexural test and 30 specimens were tested in compression.
The results were determined under the assumption of general elastic–brittle behavior of the masonry wall loaded in tension. The average value of the tensile strength—fm,t—was approximately 3.66 MPa, while the average value of the compressive strength—fm,c—was 18.61 MPa. The computed standard deviations (σflexural = 0.80; σcompresion = 1.18) indicate that the values tend to be close to the mean. Thus, it can be concluded that the experimentally determined values showed no statistically significant differences.
The experimental values were introduced as input data for the mechanical characteristics of the micro non-linear 3D model defined in Section 3 of this work.
As mentioned before, two masonry panels were manufactured and tested as reference (noted with URM and TSM). The first one (URM) was left unstrengthened, as shown in Figure 2. The second reference panel (TSM) was strengthened using a traditional system consisting of a self-supporting cement mortar matrix reinforced with steel meshes of ɸ6. The two faces of the strengthening systems were connected by means of steel connectors of ɸ6, passing through the URM panel and fixed at the exterior in the mortar layer. The overall configuration of the traditional strengthening system is illustrated in Figure 5. The mortar used for this strengthening approach has identical characteristics with the one that was used for the URM panel assemblage.
The remaining three URM panels were strengthened by plastering on one face (for one specimen—TRM1) or on both faces (for two specimens—TRM2 and TRM3) with a two-component ready-mixed, high ductility pozzolan-reaction mortar reinforced with an alkali-resistant (AR), pre-primed glass fiber mesh (Figure 6) [47,48].
According to the manufacturer [47], the mortar was cement-based, made by blending special admixtures and synthetic polymers in water dispersion and reinforced with glass fibers. The physical and the mechanical characteristics of the strengthening mortar as provided by the manufacturer are listed in Table 2. This mortar has adequate adhesion strength and, when hardened, it forms a compact and uniform layer that is impermeable both to water and aggressive atmospheric gases, while remaining highly permeable to water vapors. In total, 15 mortar prisms were prepared and subjected to the flexural test and the resulted 30 specimens were tested in compression (Figure 7). The average experimental value of the tensile strength—fm,t—was approximately 4.35 MPa, while the value given in the technical data sheet was equal with 8 MPa. Similarly, the average experimental value of the compressive strength—fm,c—was 19.77 MPa, while the producer indicated a minimum 25 MPa strength in compression at 28 days. The computed standard deviations (σflexural = 0.14; σcompresion = 1.21) indicate that the values tend to be close to the mean. Thus, it can be concluded that the experimentally determined values showed no statistically significant differences.
According to the technical data sheets, the producer determined the compressive and the flexural strength according to the provisions given in the Norms EN 12190 and EN 196/1 [49,50], while the experimental values mentioned above were determined according to the specifications given in the Norm EN 1015-11 [46]. For the micro non-linear 3D model, the mechanical properties were defined according to the experimentally determined values.
The textile meshes used to reinforce the mortar are part of the same custom design system for masonry strengthening. The meshes consist in multiple dry carbon high-strength fiber roving disposed in a square pattern [48]. Due to the custom configuration of the weave, the mechanical properties of these meshes are controlled so that, when applied on URM walls together with the mortar, they make up for the masonry’s lack of tensile strength and increase the overall ductility so that the shear stresses are distributed more evenly. As a result, in the event of seismic actions, the TRM strengthening system has the ability to evenly distribute the stresses and the strains over the entire surface of the URM walls, so that the dominant failure mechanism is shifted from a fragile type to a ductile one. Moreover, it should be noted that this type of TRM system has potential advantages when used on masonry historical buildings. In this frame, the system works in parallel with the existing structural elements, without influencing the distribution of the masses and the rigidity within the structures. The latter is a significant gain, particularly for seismic design, where stresses are proportional to the masses involved. The physical and mechanical properties of the mesh are listed in Table 3 [48].
As it can be observed in Figure 6, the face/faces of the TRM strengthening systems were additionally fixed with four transversal composite connectors, located on the corners, so as to ensure an improved connection to the masonry substrate and to avoid the out-of-plane failure. The composite connectors were unidirectional carbon fiber threaded inside a gauge wrapping [51]. Due to this appearance, this type of composite connectors is also referred to as cords. The physical and the mechanical characteristics of the cords, as given by the manufacturer, are listed in Table 4. The configuration of the anchors was selected according to the specification given by the manufacturer [51].
In order to achieve a full interaction among the cords and the specimens, a chemical anchor was manufactured by means of an adhesive product. A bi-component styrene-free adhesive made from polyester resin was poured so as to fill the holes through which the cords were inserted. The physical and mechanical characteristics of the adhesive, as provided by the manufacturer, are listed in Table 5 [52].

2.2. Construction Process

The URM panels were constructed of bricks with nominal dimensions of 1200 by 1200 by 115 mm. The latter were assembled by an experienced mason using a mortar made of Portland cement and sand, in the proportion and quality that are commonly used in the traditional Romanian masonry buildings (one part Portland cement to three parts sand). The thickness of both the horizontal and vertical mortar joints was 10 mm. Since the bricks were stored in indoor conditions, each unit was wetted before usage. After all the specimen’s manufacturing processes were complete, the surfaces were cleaned of dust, pollutants or loose materials by sandblasting and low-pressure water jetting.
For the second reference panel, two steel meshes of ɸ6 were disposed on each side (Figure 8). The meshes were tied together by means of transversal steel connectors of ɸ6. The attachments between the meshes and the transversal connectors were achieved by means of thin binding steel wires. Next, the surfaces of the panel were wetted and the mortar layer was overlaid so as to cover all the reinforcements. The overall thickness of the reinforcing layer was around 12 cm.
The remaining URM panels were strengthened with TRM systems. First, all the surfaces were wetted and the first layers of the strengthening mortar were overlaid. The two constituents of the mortar, component A (powder) and component B (liquid), were mixed according to the specifications of the manufacturer [47]. The final material consisted of a plastic–thixotropic blend that was applied to the panels’ surfaces with a flat metal smoothing towel.
After the first layer of the mortar was applied and while it was still wet, the meshes were placed over the surfaces of the panels. The meshes were lightly pressed down with a towel for them to adhere to the mortar. The adjacent pieces of the meshes were overlapped both widthways and lengthways by approximately 15 cm. Next, the second layer of the mortar was applied. The width of both mortar layers was approximately 5–6 mm.
In order to reduce the occurrence and development of the de-bonding phenomena and to improve the static efficiency of the system, the faces of the TRM system were tied with composite connectors [51]. For this purpose, after the mortar was cured, holes were drilled in the substrate and the loose material was removed with compressed air. Additionally, the surfaces inside the holes were also cleaned with a long-bristled brush. The protective gauze from the cords was unrolled to a length equal to the depth of the holes that were previously drilled into the panels. Before the cords were inserted into the panels, the adhesive was extruded, starting from the bottom of the holes, until the spaces were fully filled. The two components of the adhesive were automatically mixed together when the product was extruded, using a static mixer that was supplied together with the cartridges. The cords were then inserted into the adhesively filled holes and the excessive material was removed. The last remaining protective gauzes were removed and the fibers were spread over the substrate in a circular pattern. The overall diameter of the circle was approximately 25 cm. Finally, the spread fibers were embedded in a layer of mortar.
It is worth mentioning that, in the case of the URM panel strengthened only on one face, the anchoring was performed starting from the middle of the element to its face. This simulated a common situation for monumental buildings, when strengthening system needs to be applied without imposing any interventions to one side of the wall. The construction stages of the TRM1, TRM2 and TRM3 specimens are illustrated in Figure 9.

2.3. Instrumentation and Testing Procedures

The tests were performed according to the specifications given in ASTM E519/E519M—15 [53]. The latter describe a test procedure designed to determine the shear strength of masonry panels with modular dimensions of 1.2 by 1.2 m, by loading them in compression along the diagonal. Due to the loading direction, a diagonal tension failure is induced within the specimen. Thus, the specimens were carefully lifted, rotated at 450 and positioned on the transportation carriage in such a way that no disturbance was caused either to the unstrengthened or the strengthened panels (Figure 10).
The load was applied to the URM panel through a steel shoe placed at the top corner and transmitted to a similar shoe at the bottom corner (Figure 11). Each loading shoe had a loading area of 330 mm by 250 mm. A hydraulic jack with an overall capacity of 500 kN was incorporated between the clamp of the testing machine and the top loading shoe. The deformation of the specimens, elongation of diagonals and compression were monitored by four linear variable differential transducers (LVDTs), with two being placed on each face of the panel, oriented perpendicular and parallel to the loading direction (Figure 11). All the data were captured and stored using a data acquisition system (DAQ). Each test was load-controlled; thus, the load was increased monotonically at a constant speed of approximately 0.5–0.6 kN/s.

3. Numerical Approach

3.1. Introduction

Masonry is an anisotropic composite material which consists of masonry units (bricks, stone, etc.) assembled with or without mortar. The mechanical models that were developed to evaluate the structural behavior of the URM structures fall under the category of no-tension material models. From the theoretical point of view, URM walls are considered to behave as a linear elastic material when subjected to compressive stresses. However, based on the mechanical and elastic properties of the components, the mechanical model and, by default, the numerical one may be adapted from a typical linear–elastic to an elastic–plastic one.
Generally, three distinct modelling approaches can be adopted to simulate the structural behavior of a URM wall loaded in shear [54,55,56,57,58,59,60,61,62,63,64,65]. The first one, referred to as macro-modelling, consists in a continuum homogenous element that does not distinguish between the masonry units and mortar or between the individual components of the strengthening system. The macro-model is not suitable for the analysis of the URM walls strengthened by TRM plastering since, in this case, the stresses tend to converge into a narrow region along the faces of the composite transversal connectors. More specifically, the numerical macro-models are unable to account for the micro-mechanical characteristics at the interface levels. The second approach, referred to as the simplified micro-modelling, consists in a combination between micro and macro modelling techniques. The numerical model obtained by applying this approach has both continuum elements (for masonry units and mortar) and discontinuous elements (for the interface levels). This simplification can significantly reduce the computational costs. However, when the strengthening system is made of multiple materials with various mechanical and elastic properties (e.g., reinforced mortar, textile cords, reinforcing meshes, adhesives, etc.), the simplified numerical model can undervalue the overall shear response of the strengthened URM wall. On the other hand, the detailed micro-numerical approach allows us to identify and monitor the complete stress–strain state of the strengthened URM walls. These models are designed to account for each component of the physical models and for the particular properties of each material, thus reflecting the shear structural behavior of the URM walls strengthened with TRM in a more realistic manner.

3.2. Model Definition

In this study, a detailed micro non-linear 3D model was developed to accurately simulate the laboratory test conditions (Figure 12). The non-linear numerical analyses were carried out using the commercial, multi-purpose finite element software Ansys V 15.0, Ansys, PA, USA [55,56,57,58,63,64].
For the numerical 3D micro-models, the bricks and the mortar were simulated using SOLID187 tetrahedron finite elements (Figure 13a) [55]. The latter consist of higher-order 3D elements with 10 nodes, each of them defined by three degrees of freedom. These elements were selected based on their characteristic quadratic displacement behavior which can account for large deflections and significant strain variations. The components of the TRM system and the composite cords were modelled by SHELL 63 finite elements, as they possess both membrane and bending capabilities (Figure 13b). Moreover, the 3D micro-models were defined to account for three distinct interface levels (bricks–mortar, TRM–bricks, TRM–mortar). CONTA 174 bonded contact elements were modelled at each interface level so as to detect any possible contact separation between the TRM system and the URM panels (Figure 13c).
The bricks were assumed to behave as linear elastic isotropic materials and the plasticity properties were entirely assessed to the mortar, which was modelled as an elastic–plastic material. In this approach, the structural characteristics of the mortar are capable to account for the global non-linear behavior of the URM module. In addition, by applying this modelling strategy, it is assured that failure occurs in a characteristic mode, which is defined by a continuous diagonal crack that passes through the head and the bed mortar joints. The plasticity of the mortar was defined using the Drucker–Prager formulation. According to the latter, the material is characterized by a specific domain of yield stresses. When the yield surface is reached, the mortar starts to deform plastically and, upon further increase in load, the plastic flow is initiated.
As mentioned before, the complete test specimens were modelled, including the interface levels. For this purpose, the augmented Lagrange formulation was used to define the contacts. The penetration points were determined for both bricks and mortar based on the integration point detection.
Since the stresses vary with a high gradient between distinct components of the 3D model, the mesh size was set differently for bricks, mortar, TRM and composite cords. For the bricks, the maximum mesh size was limited to 30 mm; for the mortar and the composite cords, the mesh size was limited to maximum 2 mm; whereas, for the TRM system, a maximum length of 80 mm was imposed in the model (Figure 14).
The nonlinear 3D micro-detailed models were analyzed by using the Newton–Raphson iteration method. More specifically, the method was applied by gradually increasing the load, up to the limit where the convergence criterion was satisfied. Furthermore, whenever required, various sub-steps were defined so as to divide the load ratio. Thus, the final step/sub-step corresponded to the ultimate load. This value was reached at the end of the elastic branch, immediately before an abrupt change in displacement was recorded. This change also indicated that the convergence criterion was no longer satisfied.

4. Results and Discussion

In the case of the URM reference panel, the failure occurred in the mortar layer by splitting the specimen along the horizontal and vertical joints (Figure 15). Besides the typical propagation path of the crack (through the mortar layer), shortly before the force reached its ultimate value, the crack propagated even through the bricks.
By analyzing the load–displacement curve (on both faces of the panel) of the URM reference panel, depicted based on both experimentally and numerical results, it can be observed that, in the first stage, the specimen’s response was quasi-linear–elastic with almost constant stiffness value. In the second plateau of the graph, the load–displacement curve illustrates a plastic phase which represents the degraded stiffness state of the URM panel (Figure 16). The plastic behavior was recorded immediately after the first cracks had started to develop. At the end of the plastic branch, all the cracks indicated by arrows in Figure 15 were joined in a continuous crack that spanned, in the vertical direction, between the loaded corners of the masonry panel. At the end of the test, the masonry panel was separated into two parts along the direction of the crack.
As it can be observed, the numerical and the experimental results are in good agreement both for ultimate values and distributions. It should also be mentioned that a sign convention was adopted in order to represent, in the same graph, both the horizontal and vertical displacements. For the evaluation of the shear stress–shear strain state, all the data were taken as absolute values.
In the case of the TSM panel, even though the overall thickness of the strengthening systems is around 12 cm, the typical pattern for crack development (across the masonry mortar joints) can be easily identified (Figure 17). When the load reached its ultimate value, large surfaces of mortar started to expel, exposing the steel reinforcement meshes (Figure 17b). Moreover, the failure by panel splitting is evidenced by the distribution of the horizontal displacement, where it can be observed that, at a relatively constant load, or even slightly decreasing, the displacements increase largely. Two local failures were also recorded in the ranges 38–42 KN and 50–52 KN, respectively (Figure 18).
Unlike the reference URM panels, the TRM-strengthened ones (TRM1, TRM2 and TRM3) evidenced a gradual failure mode, which is highly advantageous for the masonry structures located in earthquake-vulnerable areas. For the TRM1 panel, the crack pattern is similar to the ones developed for the reference panels (Figure 19a). However, on the plastered face, the crack pattern is slightly shifted toward the borders of the circular regions where the composite connectors were embedded with the mortar (Figure 19b).
The TRM 2 and TRM3 panels developed a particular crack pattern which followed the border line of the composite anchors (Figure 20). Besides preventing the de-bonding phenomena and improving the static efficiency of the TRM system (the main functions of the composite anchors), the exterior part of the cords provided an additional reinforcement for the system. More specifically, the radial orientation of these fibers modified the crack pattern by shifting its original vertical direction towards the border region of the exterior side of the composite anchors (Figure 20b,c). Moreover, the sliding effect at the joints was negligible due to the presence of the end parts of the anchors (also referred as diatones). On the contrary, in the case of similar experimental works, that were performed on masonry panels tied with punctual transversal connectors, the sliding phenomena was more intense, as reported in [66].
As it can be observed in Figure 21, Figure 22, Figure 23, Figure 24 and Figure 25, beside the linear–elastic plateau, for all the specimens (including the URM panel strengthened only on one face), a characteristic plateau of constant load and increasing displacement was recorded. This plateau is similar to the plastic range (yield plateau) representation of structural carbon steel elements. As shown in the load–displacement curves, in the plastic stage, the load remains constant while the displacements continue to increase, meaning that the elongation and contraction continue as long as the load is not removed. In addition, this behavior indicates that the TRM systems provide significant additional ductility that enables the URM panels to largely deform before failure. Nevertheless, this behavior demonstrates the efficiency of the TRM systems that are applied only on one face of the panel, a case which often comes across in the strengthening applications of monumental masonry buildings. The anchoring techniques (both the side-to-side and the middle-to-side method) provide sufficient lateral capacity to avoid the possible out-of-plane failure.
The shear stress–shear strain distributions of all panels are presented in Figure 24 and Figure 25. According to ASTM E519/E519M—15 the shear stress is computed using Equation (1) [53].
S s = 0.707 P A n
where Ss—shear stress (MPa); P—load measured along the diagonal pattern; An—net area of the panel; A n = w + h 2 t × n ; w—width of the panel (mm); h—height of the panel (mm); t—thickness of the panel; n—the percentage of the gross area that is solid (expressed as a decimal).
According to ASTM E519/E519M—15, the shear strain is computed using Equation (2) [53].
Ɣ = Δ V + Δ H g
where Ɣ—shear strain (mm/mm); ΔV—shortening on vertical direction; ΔH—extension on horizontal direction; g—monitoring length.
As it can be observed in Figure 24 and Figure 25, for all the specimens, the shear stress–shear strain distribution curves start with a relatively steep slope and increase linearly until the beginning of the plastic range.
In the cases of the URM panel and of the traditional, strengthened panel (URM and TSM panels), in the plastic phase, a substantial degraded stiffness can be observed. On the other hand, in the cases of the TRM-strengthened panels (TRM1, TRM2 and TRM3), the deformation capacity is considerably improved and the characteristic (yield plateau) that was previously mentioned for the load–displacement distribution can be easily identified. Thus, TRM systems provide significant additional ductility that enables the shear stresses to remain constant while the shear strains continue to increase, meaning that the elongation and contraction continues as long as the load is not removed.
The maximum shear stress recorded for the URM panels strengthened on both faces (TRM2 and TRM3) were 20% higher than the one measured for the URM panel strengthened only on one face. When it comes to the numerical values, similarly, an increase of 33% was recorded for the maximum shear stress for the panels strengthened on both faces when compared to the one of the panel strengthened on one face. The experimentally obtained value for the shear strain was 23% higher for the TRM2 and TRM3 specimens when compared to the one measured for the TRM1 specimen. However, the numerical values of the shear strains were almost equal in both cases.
The ultimate values of both the shear stress and shear strain that were experimentally recorded for the TSM panel were almost equal to the ones recorded for the TRM2 and TRM3 panels. However, the structural improvement of the TSM panel was obtained by increasing the specimen overall thickness by approximately 12 cm, while the overall thickness of the TRM2 and TRM3 panels was increased by only 2 cm. Thus, the total weight of the traditional strengthened system was considerably higher than the one of the modern TRM system.
According to ASTM E519/E519M—15 [53], the modulus of rigidity—G—is computed as the ratio between the shear stress—Ss—and the shear strain—Ɣ—[53]. The stiffness of the URM panels can be evaluated by quantifying the modulus of elasticity—E. The latter can be calculated using Equation (3), where υ was adopted as 0.25, as reported in previous studies relating to similar URM panels [14,60].
E = 2 G 1 + υ
The ductility of the URM panels can be quantified by the drift ratio—δ—Equation (4).
δ u = Δ u H
where Δu—the displacement measured along the diagonal, corresponding to the ultimate load; H—height of the URM specimens.
The experimental and the numerical results are listed in Table 6.
As presented in Figure 21, Figure 22, Figure 23, Figure 24 and Figure 25, the response of all the specimens was non-linear and the post-peak behavior in the cases of the strengthened panels was characterized by a relatively gradual strain softening. The shear stiffness of the TSM panel, represented by the modulus of rigidity (G), increased by 34%, when compared to the experimentally recorded value for the URM panel. Similarly, the numerical results show an increase by 43% from the previously mentioned values. In the case of the TRM1 panel, the shear stiffness was increased by 36% (experimentally determined value) and 31% (numerically determined value), when compared to the values determined for the URM panel. The largest increase in the shear stiffness was recorded for the TRM2 and TRM3 panels (approximately 42% with respect to the experimental value and 62% with respect to the numerical value).
The ductility of the URM panel, expressed as the drift ratio, is considerably lower when compared to the values determined for the strengthened panels. Thus, increases in ductility of 64% for the TSM panel, 54% for the TRM1 panel, 66% for the TRM2 panel and 34% for the TRM3 panel were recorded with respect to the experimentally determined value of the URM panel. Similarly, increases in ductility of 73% for the TSM panel and 67% for the TRM1, TRM2 and TRM 3 panels were recorded with respect to the numerically determined value of the URM panel.

5. Conclusions

This paper presents the main outcomes of a numerical and experimental study which relates to the structural efficiency of a modern strengthening technique designed for URM panels. The latter consists of a TRM jacketing that can be applied either on one side of the wall or on both sides. The structural TRM layers can be anchored both by the side-to-side method and the middle-to-side one.
From the findings summarized above, the following can be concluded:
  • The observed damaged patterns both for the URM and TSM specimens matched the characteristic crack path, which consisted in a continuous-propagation step-like line that spread along the compressed diagonal, through the horizontal and vertical mortar joints.
  • The TRM2 and TRM3 panels developed a particular crack pattern which followed the border line of the composite anchors.
  • The TRM systems evidenced a general and significant increase in the original shear capability and ductility of the URM panel. They also enabled the URM panels to largely deform before failure.
  • The selected type of anchorage system provided sufficient lateral capacity to avoid the possible out-of-plane failure.
  • The ultimate loads that were experimentally determined increased by 53% for the TSM panel, 41% for the TRM1 panel, 56% and 57% for the TRM2 and TRM3 panels, when compared to the ultimate load recorded for the URM panel.
  • Similarly, the numerical results evidenced an increase of 56% for the ultimate load of the traditional strengthened panel, 45% for the panel plastered with TRM on one face and 57% for the 3D micro-model with TRM jacketing on both faces, when compared to the ultimate load recorded for the URM reference panel.
  • The ultimate values of the mechanical properties that were experimentally and numerically investigated were almost equal for the TSM panel and the TRM2 and TRM3 panels.
  • The numerical and the experimental results validate the efficiency of the TRM systems that are applied only on one face of the wall, a case which often comes across in the strengthening applications of monumental masonry buildings.
Although further experimental studies are required for an adequate assessment of the investigated strengthening techniques (e.g., position, dimension and number of the composite anchors) and for the validation of the micro-numerical model, the studies discussed in this paper represent a background for the general structural efficiency of the TRM strengthening systems.

Author Contributions

Conceptualization, N.Ț.; methodology, P.M.; validation, N.Ț.; formal analysis, D.U.; investigation, D.N.I. and D.U.; resources, D.N.I.; data curation, D.U. and N.Ț.; writing—original draft preparation, D.U.; writing—review and editing, N.Ț. and D.N.I.; supervision, N.Ț.; project administration, D.A.G. and R.C. All authors have read and agreed to the published version of the manuscript.

Funding

This research project was funded by “ANAGENNISI—Innovative Reuse of All Tyre Components in Concrete”, project FP7-ENV-2013-603722, PNII.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The data underlying this article will be shared on reasonable request from the corresponding author.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Papanicolaou, C.G.; Triantafillou, T.C.; Papathanasiou, M.; Karlos, K. Textile reinforced mortar (TRM) versus FRP as strengthening material of URM walls: Out-of-plane cyclic loading. Mater. Struct. 2008, 41, 143–157. [Google Scholar] [CrossRef]
  2. Casolo, S.; Sanjust, C.A. Seismic analysis and strengthening design of a masonry monument by a rigid body spring model: The “Maniace Castle” of Syracuse. Eng. Struct. 2009, 31, 1447–1459. [Google Scholar] [CrossRef]
  3. Bothara, J.K.; Dhakal, R.P.; Mander, J.B. Seismic performance of an unreinforced masonry building: An experimental investigation. Earthq. Eng. Struct. Dyn. 2010, 39, 45–68. [Google Scholar] [CrossRef]
  4. Bui, T.-L.; Si Larbi, A.; Reboul, N.; Ferrier, E. Shear behaviour of masonry walls strengthened by external bonded FRP and TRC. Compos. Struct. 2015, 132, 923–932. [Google Scholar] [CrossRef]
  5. Shabdin, M.; Zargaran, M.; Attari, N.K.A. Experimental diagonal tension (shear) test of Un-Reinforced Masonry (URM) walls strengthened with textile reinforced mortar (TRM). Constr. Build. Mater. 2018, 164, 704–715. [Google Scholar] [CrossRef]
  6. Brandonisio, G.; Mele, E.; De Luca, A. Closed form solution for predicting the horizontal capacity of masonry portal frames through limit analysis and comparison with experimental test results. Eng. Fail. Anal. 2015, 55, 246–270. [Google Scholar] [CrossRef]
  7. Cundari, G.A.; Milani, G.; Failla, G. Seismic vulnerability evaluation of historical masonry churches: Proposal for a general and comprehensive numerical approach to cross-check results. Eng. Fail. Anal. 2017, 82, 208–228. [Google Scholar] [CrossRef]
  8. Yardim, Y.; Lalaj, O. Shear strengthening of unreinforced masonry wall with different fiber mortar jacketing. Constr. Build. Mater. 2016, 102, 149–154. [Google Scholar] [CrossRef]
  9. Mosoarca, M.; Onescu, I.; Onescu, E.; Anastasiadis, A. Seismic vulnerability assessment methodology for historic masonry buildings in the near-field areas. Eng. Fail. Anal. 2020, 115, 104662. [Google Scholar] [CrossRef]
  10. Sayin, B.; Yildizlar, B.; Akcay, C.; Gunes, B. The retrofitting of historical masonry buildings with insufficient seismic resistance using conventional and non-conventional techniques. Eng. Fail. Anal. 2019, 115, 454–463. [Google Scholar] [CrossRef]
  11. Micelli, F.; Cascardi, A. Structural assessment and seismic analysis of a 14th century masonry tower. Eng. Fail. Anal. 2020, 107, 104198. [Google Scholar] [CrossRef]
  12. Vlachakis, G.; Cerveza, M.; Barbat, G.B.; Saloustros, S. Out-of-plane seismic response and failure mechanism of masonry structures using finite elements with enhanced strain accuracy. Eng. Fail. Anal. 2019, 97, 534–555. [Google Scholar] [CrossRef]
  13. Kalali, A.; Kabir, M.Z. Experimental response of double-wythe masonry panels strengthened with glass fiber reinforced polymers subjected to diagonal compression tests. Eng. Struct. 2012, 39, 24–37. [Google Scholar] [CrossRef]
  14. Mustafaraj, E.; Yardim, Y. Retrofitting damaged unreinforced masonry using external shear strengthening techniques. J. Build. Eng. 2019, 26, 100913. [Google Scholar] [CrossRef]
  15. Wood, W.A. Load Distribution of Masonry Walls Subject to Concentrated Loads over Opening; University of Pittsburgh: Pittsburgh, PA, USA, 1998. [Google Scholar]
  16. Gattesco, N.; Boem, I. Experimental and analytical study to evaluate the effectiveness of an in-plane reinforcement for masonry walls using GFRP meshes. Constr. Build. Mater. 2015, 88, 94–104. [Google Scholar] [CrossRef]
  17. Țăranu, N.; Cozmanciuc, R.; Ențuc, I.; Budescu, M.; Munteanu, V.; Isopescu, D. The behaviour of the interface between carbon fibre reinforced polymer composite plates and concrete. Rom. J. Mater. 2015, 45, 232–239. [Google Scholar]
  18. Bejan, L.; Țăranu, N.; Sârbu, A. Advanced polymeric composites with hybrid reinforcement. J. Optoelectron. Adv. Mater. 2010, 12, 1930–1934. [Google Scholar]
  19. Țăranu, N.; Banu, C.; Oprișan, G.; Budescu, M.; Munteanu, V.; Ioniță, O. Tensile characteristics of glass fibre reinforced polymeric bars. Rom. J. Mater. 2010, 40, 323–331. [Google Scholar]
  20. Ungureanu, D.; Țăranu, N.; Lupășteanu, V.; Isopescu, D.N.; Oprișan, G.; Mihai, P. Experimental and numerical investigation on adhesively bonded single lap and thick adherents joints between pultruded GFRP composite profiles. Compos. Part B Eng. 2018, 146, 49–59. [Google Scholar] [CrossRef]
  21. Bernat, E.; Gil, L.; Roca, P.; Escrig, C. Experimental and analytical study of TRM strengthened brickwork walls under eccentric compressive loading. Constr. Build. Mater. 2013, 44, 35–47. [Google Scholar] [CrossRef]
  22. Torres, B.; Ivorra, S.; Baeza, F.J.; Estevan, L.; Varona, B. Textile reinforced mortars (TRM) for repairing and retrofitting masonry walls subjected to in-plane cyclic loads. An experimental approach. Eng. Struct. 2021, 231, 111742. [Google Scholar] [CrossRef]
  23. Carozzi, F.G.; Milani, G.; Poggi, C. Mechanical properties and numerical modeling of fabric reinforced cementitious matrix (FRCM) systems for strengthening of masonry structures. Compos. Struct. 2014, 107, 711–725. [Google Scholar] [CrossRef]
  24. Papanicolaou, C.; Triantafillou, T.; Lekka, M. Externally bonded grids as strengthening and seismic retrofitting materials of masonry panels. Constr. Build. Mater. 2011, 25, 504–514. [Google Scholar] [CrossRef]
  25. da Porto, F.; Mosele, F.; Modena, C. In-plane cyclic behaviour of a new reinforced masonry system: Experimental results. Eng. Struct. 2011, 33, 2584–2596. [Google Scholar] [CrossRef]
  26. Wang, X.; Lam, C.C.; Lu, V.P. Bond behaviour of steel-TRM composites for strengthening masonry elements: Experimental testing and numerical modelling. Constr. Build. Mater. 2020, 253, 119157. [Google Scholar] [CrossRef]
  27. Blanksvärd, T.; Täljsten, B. Strengthening of concrete structures with cement based bonded composites. Nord. Concr. Res. 2008, 2, 133–154. [Google Scholar]
  28. Koutas, L.; Triantafillou, T.; Bousias, S. Analytical modeling of masonry-infilled RC frames retrofitted with textile-reinforced mortar. J. Compos. 2014, 19, 1–14. [Google Scholar] [CrossRef]
  29. Ismail, N.; Ingham, J.M. In-plane and out-of-plane testing of unreinforced masonry walls strengthened using polymer textile reinforced mortar. Eng. Struct. 2016, 118, 167–177. [Google Scholar] [CrossRef]
  30. Ismail, N.; Ingham, J.M. Polymer textiles as a retrofit material for masonry walls. Proc. Inst. Civ. Eng.-Struct. Build. 2014, 167, 15–25. [Google Scholar] [CrossRef]
  31. Sagar, S.L.; Singhal, V.; Rai, D.C.; Gudur, P. Diagonal shear and out-of-plane flexural strength of fabric-reinforced cementitious matrix-strengthened masonry wallets. J. Compos. Constr. 2017, 21, 04017016. [Google Scholar] [CrossRef]
  32. Marcari, G.; Basili, M.; Vestroni, F. Experimental investigation of tuff masonry panels reinforced with surface bonded basalt textile-reinforced mortar. Compos. Part B Eng. 2017, 108, 131–142. [Google Scholar] [CrossRef]
  33. Prota, A.; Marcari, G.; Fabbrocino, G.; Manfredi, G.; Aldea, C. Experimental in plane behaviour of tuff masonry strengthened with cementitious matrix-grid composites. J. Compos. Constr. 2006, 10, 1081–1097. [Google Scholar] [CrossRef]
  34. Kouris, L.A.S.; Triantafillou, T.C. State-of-the-art on strengthening of masonry structures with textile reinforced mortar (TRM). Constr. Build. Mater. 2018, 188, 1221–1233. [Google Scholar] [CrossRef]
  35. Ferrara, G.; Coppola, B.; Di Maio, L.; Incarnato, L.; Martinelli, E. Tensile strength of flax fabrics to be used as reinforcement in cement-based composites: Experimental tests under different environmental exposures. Compos. Part B Eng. 2019, 168, 511–523. [Google Scholar] [CrossRef]
  36. Ferrara, G.; Martinelli, E. Tensile behaviour of Textile Reinforced Mortar composite systems with flax fibres. In Proceedings of the 12th Fib International PhD Symposium in Civil Engineering, Prague, Czech Republic, 29–31 August 2018; Volume 29, pp. 1–7. [Google Scholar]
  37. Papanicolaou, C.G.; Triantafillou, T.C.; Karlos, K.; Papathanasiou, M. Textile reinforced mortar (TRM) versus FRP as strengthening material of URM walls: In-plane cyclic loading. Mater. Struct. 2007, 40, 1081–1097. [Google Scholar] [CrossRef]
  38. Faella, C.; Martinelli, E.; Nigro, E.; Paciello, S. Shear capacity of masonry walls externally strengthened by a cement-based composite material: An experimental campaign. Constr. Build. Mater. 2010, 24, 84–93. [Google Scholar] [CrossRef]
  39. Augenti, N.; Parisi, F.; Prota, A.; Manfredi, G. In-plane lateral response of a full scale masonry subassemblage with and without an inorganic matrix-grid strengthening system. J. Compos. Constr. 2011, 15, 578–590. [Google Scholar] [CrossRef]
  40. Parisi, F.; Iovinella, I.; Balsamo, A.; Augenti, N.; Prota, A. In-plane behaviour of tuff masonry strengthened with inorganic matrix-grid composites. Compos. Part B Eng. 2013, 45, 1657–1666. [Google Scholar] [CrossRef]
  41. Longo, F.; Cascardi, A.; Lassandro, P.; Aielo, M.A. Energy and seismic drawbacks of masonry: A unified retrofitting solution. J. Build. Pathol. Rehabil. 2021, 6, 1–24. [Google Scholar] [CrossRef]
  42. Donnini, J.; Maracchini, G.; Lenci, S.; Corinaldesi, V.; Quagliarini, E. TRM reinforced tuff and fired clay brick masonry: Experimental andanalytical investigation on their in-plane and out-of-plane behavior. Constr. Build. Mater. 2021, 272, 121643. [Google Scholar] [CrossRef]
  43. Ferrara, G.; Caggegi, C.; Martinelli, E.; Gabor, A. Shear capacity of masonry walls externally strengthened using Flax-TRM composite systems: Experimental tests and comparative assessment. Construct. Build. Mater. 2020, 261, 120490. [Google Scholar] [CrossRef]
  44. Sistem Complet de Zidărie Ceramic. Available online: https://www.wienerberger.ro/content/dam/wienerberger/romania/marketing/documents-magazines/brochures/Wienerberger_Catalog_Porotherm_2021.pdf (accessed on 19 November 2021).
  45. Partea 1: Determinarea rezistenței la compresiune. In Metode de Încercare a Elementelor Pentru Zidărie; SR EN 772-1+A1:2016; SAI Global Standards: Chicago, IL, USA, 2016. (In Romanian)
  46. Methods of Test for Mortar for Masonry. Determination of Flexural and Compressive Strength of Hardened Mortar; EN 1015-11:2019; BSI Standards: London, UK, 2019.
  47. Planitop HDM Maxi—Technical Data Sheet, 1065–3. 2019. Available online: https://www.mapei.com/ae/en/products-and-solutions/products/detail/planitop-hdm-maxi (accessed on 14 November 2021).
  48. Mapegrid C 170—Technical Data Sheet, 1025–1026. 2019. Available online: https://www.mapei.com/it/en/products-and-solutions/products/detail/mapegrid-c-170 (accessed on 14 November 2021).
  49. Products and Systems for the Protection and Repair of Concrete Structures. Test Methods. Determination of Compressive Strength of Repair Mortar. EN 12190:1999. Available online: https://standards.iteh.ai/catalog/standards/cen/4191a705-4001-4412-ae57-f21e7994bb79/en-12190-1998 (accessed on 14 November 2021).
  50. Methods of Testing Cement. Determination of Strength. EN 196-1:2016. Available online: https://standards.iteh.ai/catalog/standards/cen/37b8816e-4085-4dcc-a642-a383d9bddd6c/en-196-1-2016 (accessed on 14 November 2021).
  51. MapeWrap C Fiocco—Technical Data Sheet, 1012/1017/1026-8. 2019. Available online: https://www.mapei.com/nz/en/products-and-solutions/products/detail/mapewrap-c-fiocco (accessed on 14 November 2021).
  52. Mapefix PE Wall—Technical Data Sheet, 5803/10. 2012. Available online: https://www.mapei.com/it/en/products-and-solutions/products/detail/mapefix-pe-sf (accessed on 14 November 2021).
  53. Standard Test Method for Diagonal Tension (Shear) in Masonry Assemblages; ASTM E519/E519M-15; ASTM International: West Conshohocken, PA, USA, 2021.
  54. Ghiga, D.A.; Țăranu, N.; Ungureanu, D.; Isopescu, D.N.; Scutaru, M.C.; Hudișteanu, I. Numerical modelling of structural behaviour of URM panels strengthened with cement matrix composites. IOP Conf. Ser. Mater. Sci. Eng. 2019, 591, 012037. [Google Scholar] [CrossRef] [Green Version]
  55. Drougkas, A.; Roca, P.; Molins, C. Experimental analysis and detailed micro-modeling of masonry walls subjected to in-plane shear. Eng. Fail. Anal. 2019, 95, 82–95. [Google Scholar] [CrossRef]
  56. Hudisteanu, I.; Țăranu, N.; Isopescu, D.N.; Bejan, L.; Axinte, A.; Ungureanu, D. Improving the mechanical properties of composite laminates through the suitable selection of the corresponding materials and configurations. Rom. J. Mater. 2017, 47, 252–266. [Google Scholar]
  57. Ungureanu, D.; Țăranu, N.; Isopescu, D.N.; Lupășteanu, V.; Mihai, P.; Hudișteanu, I. Analytical and numerical study of adhesively bonded composite pultruded elements. Rom. J. Mater. 2017, 47, 522–531. [Google Scholar]
  58. Ghiga, D.A.; Țăranu, N.; Ungureanu, D.; Isopescu, D.N.; Oprișan, G.; Hudișteanu, I. IOP Conference Series—Materials Science and Engineering, Modtech International Conference—Modern Technologies in Industrial Engineering VIII; IOP Publishing Ltd.: Bristol, UK, 2020; Volume 916, p. 012041. [Google Scholar]
  59. Halabian, A.M.; Mirshahzadeh, L.; Hashemol-Hosseini, H. Non-linear behaviour of unreinforced masonry walls with different Iranian traditional brick-work settings. Eng. Fail. Anal. 2014, 44, 46–65. [Google Scholar] [CrossRef]
  60. Karaton, M.; Aksoy, H.S.; Sayin, E.; Calayir, Y. Nonlinear seismic performance of a 12th century historical masonry bridge under different earthquake levels. Eng. Fail. Anal. 2017, 79, 408–421. [Google Scholar] [CrossRef]
  61. Scacco, J.; Grillanda, N.; Milani, G.; Lourenco, P.B. Novel non-linear static numerical model for curved masonry structures based on a combined adaptive limit analysis and discrete FE computations. Int. J. Solids Struct. 2022, 236–237, 111265. [Google Scholar] [CrossRef]
  62. Pineda, P. Collapse and upgrading mechanisms associated to the structural materials of a deteriorated masonry tower. Nonlinear assessment under different damage and loading levels. Eng. Fail. Anal. 2016, 63, 72–93. [Google Scholar] [CrossRef]
  63. Nelson, T.; Wang, E. Reliable FE-Modeling with ANSYS (Ansys Support Data Base). Available online: https://support.ansys.com/staticassets/ANSYS/staticassets/resourcelibrary/confpaper/2004-Int-ANSYS-Conf-24.PDF (accessed on 1 June 2021).
  64. Ansys Courses. Available online: https://www.sharcnet.ca/Software/Ansys/15.0.7/enus/help/ans_thry/thy_el174.html (accessed on 1 June 2021).
  65. Mustafaraj, E.; Yardim, Y. Usage of ferrocement jacketing for strengthening of damaged unreinforced masonry (URM) walls. In Proceedings of the 3rd International Balkans Conference on Challenges of Civil Engineering, Tirana, Albania, 19–21 May 2016; pp. 153–163. [Google Scholar]
  66. Casardi, A.; Leone, M.; Aielo, M.A. Transversal joining of multi-leaf masonry through different types of connector: Experimental and theoretical investigation. Constr. Build. Mater. 2020, 272, 120733. [Google Scholar] [CrossRef]
Figure 1. Brick unit (dimensions in mm) [44].
Figure 1. Brick unit (dimensions in mm) [44].
Materials 14 07021 g001
Figure 2. Specimens: (a) geometric configuration (values in mm) and (b) URM craftmanship.
Figure 2. Specimens: (a) geometric configuration (values in mm) and (b) URM craftmanship.
Materials 14 07021 g002
Figure 3. Brick unit tested in compression using a WAW 600 Universal Testing Machine.
Figure 3. Brick unit tested in compression using a WAW 600 Universal Testing Machine.
Materials 14 07021 g003
Figure 4. Flexural test: (a) mortar prism specimen and (b) failure mode. Compression test: (c) specimen and (d) failure mode.
Figure 4. Flexural test: (a) mortar prism specimen and (b) failure mode. Compression test: (c) specimen and (d) failure mode.
Materials 14 07021 g004
Figure 5. Configuration of the traditional strengthening system—TSM panel.
Figure 5. Configuration of the traditional strengthening system—TSM panel.
Materials 14 07021 g005
Figure 6. Configuration of the TRM strengthening system.
Figure 6. Configuration of the TRM strengthening system.
Materials 14 07021 g006
Figure 7. Flexural test: (a) mortar prism specimen and (b) failure mode. Compression test: (c) specimen and (d) failure mode.
Figure 7. Flexural test: (a) mortar prism specimen and (b) failure mode. Compression test: (c) specimen and (d) failure mode.
Materials 14 07021 g007
Figure 8. (a) TSM panel and (b) transversal connector.
Figure 8. (a) TSM panel and (b) transversal connector.
Materials 14 07021 g008
Figure 9. Construction stages: (a) application of the first layer of mortar and reinforcing meshes; (b) overlap of the reinforcing meshes; (c) insertion of composite cords; (d) cords spreading in a circular pattern; (e) embedment of the cords with mortar; (f) surface levelling and final checks.
Figure 9. Construction stages: (a) application of the first layer of mortar and reinforcing meshes; (b) overlap of the reinforcing meshes; (c) insertion of composite cords; (d) cords spreading in a circular pattern; (e) embedment of the cords with mortar; (f) surface levelling and final checks.
Materials 14 07021 g009
Figure 10. Specimen positioned on the transportation carriage: (i) loading shoe and (ii) transportation carriage.
Figure 10. Specimen positioned on the transportation carriage: (i) loading shoe and (ii) transportation carriage.
Materials 14 07021 g010
Figure 11. Specimen instrumentation and loading conditions: 1—URM wall; 2—loading shoe; 3—loading jack; 4—loading cell; 5—LVDTs; 6—steel channel.
Figure 11. Specimen instrumentation and loading conditions: 1—URM wall; 2—loading shoe; 3—loading jack; 4—loading cell; 5—LVDTs; 6—steel channel.
Materials 14 07021 g011
Figure 12. Three-dimensional model: 1—URM panel; 2—Planitop HDM Maxi mortar; 3—Mapegrid C 170 meshes; 4—MapeWrap C Fiocco composite connectors.
Figure 12. Three-dimensional model: 1—URM panel; 2—Planitop HDM Maxi mortar; 3—Mapegrid C 170 meshes; 4—MapeWrap C Fiocco composite connectors.
Materials 14 07021 g012
Figure 13. Finite elements: (a) SOLID187, (b) SHELL 63 and (c) CONTA174. *i, j, k, l, m, n, o, p, q, r—nodes; MX, Y, XY—bending moments; SX, Y—displacements. Figure adapted from [59].
Figure 13. Finite elements: (a) SOLID187, (b) SHELL 63 and (c) CONTA174. *i, j, k, l, m, n, o, p, q, r—nodes; MX, Y, XY—bending moments; SX, Y—displacements. Figure adapted from [59].
Materials 14 07021 g013
Figure 14. Finite element mesh of (a) URM panel and (b) URM panel strengthened with TRM.
Figure 14. Finite element mesh of (a) URM panel and (b) URM panel strengthened with TRM.
Materials 14 07021 g014
Figure 15. (a) URM panel loaded into the testing machine; (b) Failure mode—crack propagation pattern through the mortar joints.
Figure 15. (a) URM panel loaded into the testing machine; (b) Failure mode—crack propagation pattern through the mortar joints.
Materials 14 07021 g015
Figure 16. Load–displacement distribution for the URM panel.
Figure 16. Load–displacement distribution for the URM panel.
Materials 14 07021 g016
Figure 17. (a) Failure mode of the TSM panel and (b) detail of A-A.
Figure 17. (a) Failure mode of the TSM panel and (b) detail of A-A.
Materials 14 07021 g017
Figure 18. Load–displacement distribution for the TSM panel.
Figure 18. Load–displacement distribution for the TSM panel.
Materials 14 07021 g018
Figure 19. URM panel strengthened with TRM on one face (TRM1 panel). (a) Unstrengthened face: (i) crack propagation through mortar joints and (ii) crack propagation through brick units; (b) Strengthened face: (iii) crack propagation close to the composite anchors.
Figure 19. URM panel strengthened with TRM on one face (TRM1 panel). (a) Unstrengthened face: (i) crack propagation through mortar joints and (ii) crack propagation through brick units; (b) Strengthened face: (iii) crack propagation close to the composite anchors.
Materials 14 07021 g019
Figure 20. TRM2 and TRM 3 panels. (a) Crack pattern. (b) Detail of A-A: (i) exterior side of the composite anchors. (c) Detail of B-B: (ii) exposed composite cords and (iii) failure of the TRM by fiber mesh rupture.
Figure 20. TRM2 and TRM 3 panels. (a) Crack pattern. (b) Detail of A-A: (i) exterior side of the composite anchors. (c) Detail of B-B: (ii) exposed composite cords and (iii) failure of the TRM by fiber mesh rupture.
Materials 14 07021 g020
Figure 21. Load–displacement distribution for the URM panel strengthened with TRM on one face (TRM1 panel).
Figure 21. Load–displacement distribution for the URM panel strengthened with TRM on one face (TRM1 panel).
Materials 14 07021 g021
Figure 22. Load–displacement distribution for the URM specimen strengthened with TRM on both faces (TRM2 panel).
Figure 22. Load–displacement distribution for the URM specimen strengthened with TRM on both faces (TRM2 panel).
Materials 14 07021 g022
Figure 23. Load–displacement distribution for the URM specimen strengthened with TRM on both faces (TRM3 panel).
Figure 23. Load–displacement distribution for the URM specimen strengthened with TRM on both faces (TRM3 panel).
Materials 14 07021 g023
Figure 24. Shear stress–shear strain distributions: experimental results.
Figure 24. Shear stress–shear strain distributions: experimental results.
Materials 14 07021 g024
Figure 25. Shear stress–shear strain distributions: numerical results.
Figure 25. Shear stress–shear strain distributions: numerical results.
Materials 14 07021 g025
Table 1. In-plane tests of URM panels strengthened with TRM [34].
Table 1. In-plane tests of URM panels strengthened with TRM [34].
AuthorsTest TypeNo. of PanelsType of MasonryType of Reinforcing MeshesNo. of Strengthened SidesFailure MechanismStrength RatioDeformation Ratio
Prota et al., 2006 [33]DG4TFG1Tensile rupture1.72.4
Prota et al., 2006 [33]DG4TFG2Crushing2.22.3
Papanicolaou et al., 2007 [37]SH4BRC2Crushing8.213.5
Crushing2.54.2
Debonding and crushing5.37.2
Faella et al., 2010 [38]DG9TFC1Debonding and crushing5.7---
Augenti et al., 2011 [39]CY1BRG1Tensile rupture1.032.8
Parisi et al., 2013 [40]DG6TFG1/2Tensile rupture2.42.7
Ismail and Ingham, 2016 [29]CY1BRS1Tensile rupture1.21.2
Marcari et al., 2017 [32]DG3TFB1Vertical cracks1.32.4
Marcari et al., 2017 [32]DG2TFB2Vertical cracks1.61.6
Sagar et al., 2017 [31]DG15BRG1Tensile rupture1.037.2
Longo et al., 2021 [41]DG2BRG2Vertical cracks1.6-
Longo et al., 2021 [41]DG2BRS2Tensile rupture1.7-
Donnini et al., 2021 [42]DG3TFG2Vertical cracks2.74.0
Donnini et al., 2021 [42]DG3BRG2Vertical cracks1.31
Table 2. Physical and mechanical characteristics of the strengthening mortar (provided by the manufacturer) [47].
Table 2. Physical and mechanical characteristics of the strengthening mortar (provided by the manufacturer) [47].
Consistency of mixPlastic–thixotropic
Density of wet mix (kg/m3)1850
CoatingEpoxy–Silicone–PFT–Titanium
Workability (h)1
Water absorption (kg/(m2·min0.5)≤0.1
Thermal conductivity (W/m·K)0.73
Compressive strength (MPa)25 (after 28 days)
Flexural strength (MPa)8 (after 28 days)
Compressive modulus of elasticity (MPa)10,000 (after 28 days)
Initial shear strength (MPa)0.15
Table 3. Physical and mechanical characteristics of the mesh (provided by the manufacturer) [48].
Table 3. Physical and mechanical characteristics of the mesh (provided by the manufacturer) [48].
Type of FiberHigh-Strength Carbon Fiber
Weight (g/m2)170
Mesh size (mm)10 × 10
Density (kg/m3)1830
Tensile strength (MPa)4800
Modulus of elasticity (MPa)230,000
Load-resistant area per unit of width (mm2/m)48
Equivalent thickness of dry fabric (mm)0.048
Elongation at failure (%)2
Table 4. Physical and mechanical characteristics of the cords (provided by the manufacturer) [51].
Table 4. Physical and mechanical characteristics of the cords (provided by the manufacturer) [51].
Type of FiberHigh-Strength Carbon Fiber
Appearancecord
Density (kg/m3)1800
Equivalent surface area of dry fabric (mm2)21.24
Modulus of elasticity (MPa)230,000
Tensile strength (MPa)4830
Elongation at failure (%)2
Table 5. Physical and mechanical characteristics of the ɸ8 mm cords (provided by the manufacturer) [52].
Table 5. Physical and mechanical characteristics of the ɸ8 mm cords (provided by the manufacturer) [52].
AppearanceThixotropic Paste
Density (kg/m3)1690
Compressive strength (MPa)68
Flexural strength (MPa)30
Flexural dynamic modulus of elasticity (MPa)4025
Compressive modulus of elasticity (MPa)6105
Table 6. Summary of experimental and numerical results.
Table 6. Summary of experimental and numerical results.
CharacteristicsURM TSMTRM1TRM2TRM3
Pult_exp (kN)25.43254.37843.02458.69559.364
Pult_num (kN)24.90057.21045.15558.34558.345
Ss_exp (MPa)0.0430.1570.1140.1670.137
Ss_num (MPa)0.0420.1380.1140.1520.152
Ɣexp (mm/mm)0.0070.0170.0120.0150.012
Ɣnum (mm/mm)0.0080.0150.0150.0140.014
Gexp (MPa)6.1429.2359.50011.13311.417
Gnum (MPa)5.2509.2007.60010.85710.857
Eexp (MPa)15.35523.08823,75027.83328.542
Enum (MPa)13.12523.00019.00027.14328.843
δu_exp (%)0.2200.6090.4730.6500.331
δu_num (%)0.2360.8840.7070.7070.707
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Ungureanu, D.; Țăranu, N.; Ghiga, D.A.; Isopescu, D.N.; Mihai, P.; Cozmanciuc, R. Diagonal Tensile Test on Masonry Panels Strengthened with Textile-Reinforced Mortar. Materials 2021, 14, 7021. https://doi.org/10.3390/ma14227021

AMA Style

Ungureanu D, Țăranu N, Ghiga DA, Isopescu DN, Mihai P, Cozmanciuc R. Diagonal Tensile Test on Masonry Panels Strengthened with Textile-Reinforced Mortar. Materials. 2021; 14(22):7021. https://doi.org/10.3390/ma14227021

Chicago/Turabian Style

Ungureanu, Dragoș, Nicolae Țăranu, Dan Alexandru Ghiga, Dorina Nicolina Isopescu, Petru Mihai, and Ruxandra Cozmanciuc. 2021. "Diagonal Tensile Test on Masonry Panels Strengthened with Textile-Reinforced Mortar" Materials 14, no. 22: 7021. https://doi.org/10.3390/ma14227021

APA Style

Ungureanu, D., Țăranu, N., Ghiga, D. A., Isopescu, D. N., Mihai, P., & Cozmanciuc, R. (2021). Diagonal Tensile Test on Masonry Panels Strengthened with Textile-Reinforced Mortar. Materials, 14(22), 7021. https://doi.org/10.3390/ma14227021

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop