Next Article in Journal
Radiative Thermal Effects in Large Scale Additive Manufacturing of Polymers: Numerical and Experimental Investigations
Next Article in Special Issue
Elimination of Composition Segregation in 33Al–45Cu–22Fe (at.%) Powder by Two-Stage High-Energy Mechanical Alloying
Previous Article in Journal
Crystal Structure and Concentration-Driven Phase Transitions in Lu(1−x)ScxFeO3 (0 ≤ x ≤ 1) Prepared by the Sol–Gel Method
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

In Situ Ti6Al4V/TiB Composites Prepared by Hydrogen-Assisted Sintering of Blends Containing TiH2 and Ball-Milled Ti+TiB2 Powders

1
College of Materials Science and Engineering, Jilin University, Changchun 130025, China
2
International Center of Future Science, Jilin University, Changchun 130025, China
3
G.V. Kurdyumov Institute for Metal Physics, 03115 Kyiv, Ukraine
*
Author to whom correspondence should be addressed.
Materials 2022, 15(3), 1049; https://doi.org/10.3390/ma15031049
Submission received: 6 January 2022 / Revised: 26 January 2022 / Accepted: 27 January 2022 / Published: 29 January 2022
(This article belongs to the Special Issue Powder Metallurgy: Materials and Processing)

Abstract

:
In the present study, 98.6–99.5% dense in situ reinforced Ti6Al4V/TiB composites were manufactured with a newly developed approach based on hydrogen-assisted blended elemental powder metallurgy (BEPM). The approach includes the activation milling of titanium powder produced with hydrogenation-dehydrogenation (HDH-Ti powder) with finer TiB2 additives, following blending with TiH2 and master alloy (MA) powders, and final press-and-sinter operations. Scanning electron microscope (SEM) observations prove the formation of microstructures with improved density and homogeneous distribution of TiB reinforcements in a sintered Ti6Al4V matrix. Hardness and compressive tests validated the high mechanical characteristics of produced composites. The effect of preliminary milling time over 2–6 h and the ratio of hydrogenated and non-hydrogenated titanium powders used (TiH2 vs. HDH Ti) on microstructure and mechanical properties were studied to further optimize the processing parameters. Test results indicate the above approach can be regarded as a promising route for the cost-effective manufacturing of Ti6Al4V/TiB composite with reduced porosity, tailored microstructure uniformity, acceptable impurity level and, hence, mechanical characteristics sufficient for practice applications.

1. Introduction

Metal matrix composites are the subject of numerous studies [1,2,3,4,5,6]. Particle-reinforced titanium matrix composites (PRTMCs) have been widely studied and have proved to be excellent materials for critical applications such as aerospace, defense and medical instruments due to isotropic homogeneity, improved modulus and high-temperature characteristics [1]. Among various reinforcements for such titanium-based composites, in situ formed TiB has been deemed as one of the reinforcements with the most potential owing to its high Young modulus, elevated specific strength, brilliant thermal stability and clean and strong metallurgical bonding interface with matrix [2,3]. Therefore, intensive efforts have been performed on manufacturing PRTMCs reinforced with in situ formed TiB.
Compared with other manufacturing routes, Blended Elemental Powder Metallurgy (BEPM) provides a bottom cost level for PRTMC processing [4,5,6,7], especially if desirable microstructure and characteristics can be achieved with the simplest press-and-sinter option without using complicated and expensive technologies such as hot isostatic pressing [8,9] and spark plasma sintering (SPS) [10,11,12]. It has been demonstrated that using titanium hydride (TiH2) powder instead of titanium powder in the starting blends brings some advantages for the simple press-and-sinter production of PRTMCs. Using titanium hydride as a starting powder further promotes the cost-effectiveness of the BEPM manufacturing route, while TiH2 dehydrogenation with the emission of atomic hydrogen on vacuum heating can clean the powder surfaces, reducing the content of O, C and Cl in the final material [13]. Moreover, phase transformation of titanium hydride into dehydrogenated titanium induces the acceleration of diffusion and powder sintering activation. Unfortunately, for BEPM manufacturing of composites reinforced with in situ formed TiB particles, a positive influence of TiH2→Ti transformation on activated densification usually is not observed. The employment of raw TiB2 or B powders as the boron source in BEPM processing resulted in the formation of excessive residual porosity in the titanium-based matrix during Ti+TiB2→TiB or Ti+B→TiB reactions and inhomogeneous partially reacted reinforcements in sintered microstructures [14,15,16]. Another problem is that the achievement of fine TiB precipitations in sintered composites, because of coarse raw TiB2 particles or their agglomerations formed during powder preparation procedures, cannot be easily fractionized into dispersed ones. To improve the mechanical performance of composites, reduction of residual porosity and formation of fine boride reinforcements evenly distributed over the matrix is necessary. For the desirable modification of composite microstructure, application of hot isostatic pressing during sintering and post-sintering thermal mechanical processing should be performed. However, these extra procedures definitely bring unwanted increase in material cost. Previous work by current authors indicates that the hydrogen-assisted 2 stage press-and-sintering route can effectively transform the porous composites into nearly dense materials without hot pressing or hot deformation operations, but doubled powder preparation, compaction and sintering procedures induce risks for material contamination with atmospheric impurities and degraded ductile properties [17].
To achieve enhanced sintered densities (reduced porosities) of BEPM-produced titanium alloys, preliminary activation of raw powders or powder blends by milling can be successfully used [18,19,20]. The same treatment is a potential way to improve sintered microstructures of TiB reinforced composites. However, activation milling simultaneously increases the risk of powder contamination, which requires the proper selection of processing parameters to attain desirable characteristics of the final material.
The main aim of the present study is to develop a cost-effective hydrogen-assisted BEPM press-and-sinter approach ensuring the formation of nearly dense composites on the base of a Ti6Al4V alloy matrix with uniformly distributed TiB particles and acceptable impurity contents. To achieve desirable characteristics during pressureless sintering, activation milling of powders was included in the processing. The impact of processing parameters on microstructure and mechanical properties of the produced composites is investigated to demonstrate the potential of the practice application of such a manufacturing approach.

2. Materials and Methods

In the present research, BEPM production of composite on the base of a Ti6Al4V (wt%) alloy matrix reinforced with 5 vol.% of TiB phase was studied. Two kinds of powders, having different physical and mechanical characteristics, namely, TiH2 and HDH-Ti powders, were used together as the titanium base of powder blends. Titanium sponge (Baoti Huashen Titanium Industry Co., Ltd., Xi’an, China) was used as a starting material to produce both abovementioned powders. The sponge was hydrogenated up to a concentration of 3.5 wt% H (close to TiH2 composition) using heating to 600 °C and subsequent cooling to 300 °C under a hydrogen atmosphere. Then, the hydrogenated sponge was ball milled by a planetary milling device (QM-QX2, Nanda Instrument Plant, Nanjing, China) and sieved with 88 μm cell screen to obtain a TiH2 powder less than 88 µm in particle size. HDH-Ti powder (particle size 45–88 μm) was obtained by dehydrogenation of TiH2 powder (less than 88 µm) and 2nd sieving using a 45 µm screen to select desirable powder sizes. Apart from the above-noted two kinds of titanium source, relatively fine 60%Al-40%V master alloy (MA) (~10 μm) and TiB2 (~10 μm) powders (Futaiyuan metal materials Co., Ltd., Baoji, China) were used as starting materials. Figure 1 shows the actual morphology of the abovementioned raw powder particles based on SEM observations, while the impurity contents in raw materials are listed in Table 1.
Quite different characteristics of TiH2 and HDH Ti powders were profitably used in the manufacturing process of the Ti6Al4V-5%TiB composite to achieve a desirable, nearly dense and uniform microstructure. In various experiments (Table 2), an amount of TiB2 powder corresponding to 5 vol% TiB phase in final composite was preliminary ball milled for 2/4/6 h at 200 rpm together with various amounts of HDH Ti powder using a 5:1 ball to powder ratio. Despite the fact that ductile HDH Ti particles demonstrate a low tendency for size reduction with milling, it was assumed that the milling operation enables their severe plastic deformation and the covering of the surface of relatively large titanium particles with finer TiB2 ones. The close and tight bonding between TiB2 and HDH-Ti powders formed during milling should promote the activation of an in situ Ti+TiB2→TiB reaction at interfaces during the heating cycle and presumably suppress the formation of porosity. In contrast, brittle and low-strength TiH2 particles can be easily fragmented during milling, but the irregular morphology of hydride fragments (like that shown in Figure 1b) should not provide their close contact with TiB2 particles during milling and subsequent compaction. Moreover, intensive milling significantly increases the oxygen content in TiH2 powder [21]. For these reasons, preliminary activation milling of TiH2 powder was rejected. As was shown earlier, a positive contribution of titanium hydride to densification improvement can be achieved even without milling, owing to the additional fragmentation of TiH2 particles on compaction [22,23] and to the phase transformation of δ-TiH2 to β-Ti and α Ti on further vacuum sintering, which creates huge amounts of crystal lattice defects promoting the activation of diffusion as well as the homogenization and sintering of powder compacts controlled by diffusion [24]. Taking into consideration the above-described ideas, preliminary milled HDH-Ti+TiB2 powders were blended with corresponding amounts of TiH2 powder (Table 1) as well as Al-V MA powder to achieve total Ti6Al4V-5vol%TiB composition of each BEPM sample, while each sample (powder blend) was characterized with a definite TiH2-HDH-Ti ratio. To highlight the role of the individual TiH2 powder without the milling operation and, in contrast, the individually milled HDH Ti powder in the processing, blends 4 and 7, correspondingly, (Table 1) were prepared and tested. Powders were blended together for 6 h under argon atmosphere protection; powder blends were subsequently die-compacted at 600 MPa and sintered under vacuum at 1250 °C for 4 h to transform BEPM compacts into dehydrogenated bulk composites.
The effects of the processing parameters, including variation in milling time and different proportions of HDH-Ti used in the milling stage to TiH2 additions in the blending stage, on microstructural and mechanical characteristics of sintered composites were studied and corresponding samples were listed in Table 1.
Scanning electron microscopy under both secondary electron (SE) and backscattered electron (BSE) modes (SEM, JSM-IT500A, JEOL Ltd., Tokyo, Japan) was adopted for microstructure observation. Phase composition was identified using X-ray diffraction (XRD, Rigaku, Tokyo, Japan) (CuKa, λ = 0.15406 nm). Residual porosity was calculated as the ratio of actual density values measured following Archimedes’ method and theoretical density (4.44 g/cm3) of the composite. Hardness was determined using a HV 1000-IS hardness tester (Nuoen Ltd., Hangzhou, China) under the load of 1000 N holding for 10 s. Compressive tests were performed on cylindrical samples (6 mm in diameter and 9 mm in height) using an automatic universal testing machine at a constant crosshead speed of 1 µm/s. Oxygen contents in powders and in sintered composites were measured with a LECO ONH 836 analyzer (LECO Instruments Co., Ltd., St. Joseph City, AZ, USA). Each of the abovementioned tests was performed at least three times to validate the test results.

3. Results and Discussion

X-ray diffraction patterns of powder blends after varied preliminary milling time and corresponding sintered composites were shown in Figure 2. The presence of α-Ti (for HDH-Ti powder), TiH2 and TiB2 diffraction peaks without traces of boride intermediate phases for all powder blends indicates that no reaction between TiB2 and the matrix occurred even with the longest milling of 6 h. The absence of TiH2 and TiB2 peaks for all sintered composites (Figure 2D–F) reveals that TiH2 was totally dehydrogenated, while a α + β titanium matrix was formed. Apart from the TiB phases, no intermediate boride phases can be detected via diffraction patterns of sintered samples, proving the overall in situ transformation of raw TiB2 particles into TiB reinforcements via reaction with the titanium matrix (Ti+TiB2→TiB). Comparative observations on starting powders shown in Figure 1 and power blends after milling shown in Figure 3 demonstrated that finer and satellite-like TiB2 particles were tightly bonded on the surface of large HDH-Ti particles which were obviously deformed during milling. Deformed titanium particles should have an increased number of crystal lattice defects, which is useful for diffusion activation on further sintering. Moreover, preliminary milling not only is effective in the formation of close contacts between the surface of HDH Ti particles and TiB2 but also allows undesirable TiB2 agglomerations to be avoided and possibly results in the breaking of coarser TiB2 particles into finer ones with a more uniform redistribution of raw TiB2 phase over green powder blends. Changes of characteristics affected by different milling times are presented in Figure 4 and Table 3. Relatively large TiB needles distributed over the lamellar (α + β) matrix can be easily observed in sample 1, as shown in Figure 4a. However, the average length of TiB needles decreased when the milling time was increased (Table 3) from 28.7 μm for a 2 h milling (sample 1) to 21.4 μm for a 4 h milling (sample 2) and 18.9 μm for a 6 h milling (sample 3) without a noticeable difference in the cross-section size of TiB precipitations. On further sintering, diffusion redistribution of boron atoms in a titanium matrix resulted in corresponding more uniform TiB phase precipitations with a higher total number of TiB needles but which had shorter length. Furthermore, the residual porosity decreased with an extended milling time (Table 3, see samples 1–3 as an example). The composites were nearly fully consolidated in that a density of 99.5% of the theoretical value was achieved for sample 3. On the other hand, prolonged milling resulted in an increase in oxygen content which, in turn, affected hardness values (Table 3). Increased hardness of the composite was achieved with a longer milling time of HDH-Ti+TiB2 powders owing to the lower residual porosity, higher oxygen content and more uniform redistribution of TiB needles. Based on the fact that a similar porosity and TiB size were obtained for samples 2 and 3 (Table 3), the difference in their hardness (340–360 HV and 360–385 HV, correspondingly) can be explained mainly by the oxygen-induced strengthening effect.
So, an increase in preliminary milling time positively affects the uniformity of TiB reinforcement redistribution among the matrix and porosity reduction; both factors are useful for the improvement of strength and ductile characteristics. However, longer milling inevitably involves risks for the contamination of the powder blends with unwanted impurities even treated with argon protection, which is harmful for the ductile characteristics. To achieve impressive mechanical characteristics of manufactured composites, sintered materials require preservation of impurity content at the admissible level. Hence, a 4 h preliminary milling time is recommended as the optimized milling condition for the fabrication of Ti6Al4V/TiB composites with the milling-blending-sintering approach based on the overall analysis of the microstructure, hardness test results and impurity contents.
Reciprocal variations in HDH-Ti amount (used in the milling procedure) to TiH2 additions (used in the blending process) also significantly affected the characteristics of the manufactured Ti6Al4V-5%TiB composites. As shown in Figure 5a, equiaxed boride clusters surrounded with pores and coarse TiB needles were observed in the lamellar matrix for sample 4. Since neither the HDH-Ti powder nor milling process were involved for this sample, TiH2 alone was regarded as the matrix source. Apparently, a reaction between the dehydrogenated titanium matrix and coarsest TiB2 particles consumes large amounts of Ti atoms resulting in the formation of voids nearby; voids retard further reaction thus preserving the initial equiaxed morphology of not completely transformed boride particles, even though traces of residual TiB2 phase were not detected by X-ray analysis (Figure 2). Furthermore, mutual diffusion between the titanium matrix and Al-V MA particles during the homogenization of the powder blend can result in the formation of Kirkendall’s porosity, which is another possible contribution to the highest residual porosity observed (~4.3%, Table 3). In contrast, with the involvement of HDH-Ti in the milling procedure, the microstructure of samples 5–7 presents a lower porosity (1.1–1.4%, Table 3 and Figure 5b–d) with no presence of equiaxed boride clusters. So, it can be asserted that preliminary milling breaks the relatively larger TiB2 particles and agglomerations of TiB2 powders, creating close contact areas between boride and HDH-Ti particles which are sufficient for the complete Ti+TiB2→TiB reaction. The average length of reinforcing TiB needles is nearly similar for samples 5–7. It should also be mentioned that an increase in the amount of milled HDH-Ti powder with a corresponding decrease in the amount of TiH2 powder in the blend resulted in a higher oxygen content (Table 3). Sample 7, produced with a milled (HDH-Ti+TiB2) blend without titanium hydride additions, demonstrated the highest oxygen content (0.455%) as listed in Table 3 when compared with samples 2,4–6. This result once more confirmed the hydrogen cleaning effect achieved using TiH2 powder as well as the influence of the milling procedure on material contamination.
Clearly, the addition of TiH2 powder is necessary since dehydrogenation takes purification effect on all materials owing to the reaction of emitted hydrogen atoms and surface impurities. At the same time, to achieve the improved densification of powder blends, the advantages of TiH2 powder, such as the fragmentation of its particles by a compacting force and filling the voids in green compacts with small fragments [22,23] as well as activated diffusion due to the TiH2→Ti transformation [24], are less effective in the present case as compared to the activation milling of HDH-Ti+TiB2 powders (Table 3, samples 4–7). So, the separate use of either activation milling for HDH Ti+TiB2 powders (sample 7) or TiH2 powder (sample 4) resulted in compromised characteristics of sintered composites, such as an increased oxygen content and increased residual porosity, correspondingly. An acceptable combination of a highly dense sintered microstructure with evenly distributed TiB needles and admissible oxygen content was achieved when TiH2 and the activation milling of HDH-Ti+TiB2 powders were used together in various proportions of TiH2 and HDH Ti powders in the blends (Table 3, samples 2, 5, 6).
Compressive testing results confirmed this conclusion. Figure 6 shows the typical engineering compressive stress–strain curves for composites produced using powder blends with different HDH-Ti to TiH2 proportions. The highest compressive strength levels (1965 ± 35 Mpa) were demonstrated by samples 5 and 6, while sample 2 presented the best compressive strain performance (29 ± 0.7%) at a slightly lower strength value (1923 ± 33 MPa). In contrast, the individual use of either HDH Ti or TiH2 powder (samples 4 and 7) resulted in noticeably reduced strength and strain characteristics. The deviations in compressive performance can be attributed to a mutual influence of several key factors. Higher proportions of milled HDH-Ti powder promote more contacting areas between severely deformed HDH-Ti and TiB2 powders, better pore healing on sintering and reduced residual porosity useful for the improvement of strength and strain characteristics. On the other hand, the decrease of TiH2 powder amount in the powder blend inhibited the cleaning effect induced by dehydrogenation during heating cycles. The oxygen pick-up during milling also contributes to hardness and strength improvement due to the oxygen strengthening mechanism, but negatively affects compressive strain performance as shown in Figure 6. Finally, important factors for mechanical characteristics are morphology, size of TiB phase and redistribution of reinforcing particles in the Ti6Al4V alloy matrix. Relatively fine TiB needles uniformly distributed in the sintered matrix (Figure 4b and Figure 5b,c) contributed to the improved strength and strain characteristics of samples 2, 5 and 6.

4. Conclusions

In the present study, Ti6Al4V-TiB composites exhibiting up to 99.5% density were produced using powder blends based on TiH2 and HDH Ti powders with relatively simple technological operations including activation milling, blending, cold compaction and vacuum sintering. The microstructure and characteristics of the composites were investigated depending on the variation of processing parameters, and the conclusions were drawn as follows.
  • Preliminary activation milling of ductile HDH Ti powder and TiB2 particles over 2–6 h is more effective in the formation of nearly dense sintered composites than hydrogen-assisted sintering of non-milled TiH2+TiB2 powders, while application of titanium hydride provides the preservation of acceptable oxygen contents (0.31–0.35%) in sintered composites.
  • An increase in the milling time of HDH-Ti+TiB2 powders within 2–6 h is useful for the reduction of residual porosity (2.3% down to 0.5%) and formation of finer TiB precipitations uniformly redistributed over the sintered matrix, but extended milling time negatively affect impurity content.
  • Cooperative use of TiH2 and milled HDH-Ti particles as a titanium base of powder blends resulted in the improved mechanical characteristics of sintered composites. Variation of HDH-Ti-TiH2 ratio in powder blends affects residual porosity, microstructure uniformity and oxygen content of sintered composites allowing us to control their hardness and compressive characteristics.

Author Contributions

Methodology/writing—original draft preparation, Y.S.; Investigation, Y.S. and F.Q.; Data curation/Formal analysis/review and editing, D.S., X.X. and O.S.; Conceptualization/supervision/Project administration, O.I. and T.C. All authors have read and agreed to the published version of the manuscript.

Funding

This research did not receive any specific grant from funding agencies in the public, commercial, or not-for-profit sectors.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Acknowledgments

The author would like to acknowledge the support of the College of Materials Science and Engineering of Jilin University in China, International Center of Future Science of Jilin University in China, and G.V. Kurdyumov Institute for Metal Physics in Ukraine.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Falodun, O.E.; Obadele, B.A.; Oke, S.R.; Okoro, A.M.; Olubambi, P.A. Titanium-based matrix composites reinforced with particulate, microstructure, and mechanical properties using spark plasma sintering technique: A review. Int. J. Adv. Manuf. Technol. 2019, 102, 1689–1701. [Google Scholar] [CrossRef]
  2. Morsi, K. Review: Titanium–titanium boride composites. J. Mater. Sci. 2019, 54, 6753–6771. [Google Scholar] [CrossRef]
  3. Morsi, K.; Patel, V.V. Processing and properties of titanium–titanium boride (TiBw) matrix composites—A review. J. Mater. Sci. 2007, 42, 2037–2047. [Google Scholar] [CrossRef]
  4. Kumar, M.S.; Chandrasekar, P.; Chandramohan, P.; Mohanraj, M. Characterisation of titanium–titanium boride composites processed by powder metallurgy techniques. Mater. Charact. 2012, 73, 43–51. [Google Scholar] [CrossRef]
  5. Sadoun, A.M.; Mohammed, M.M.; Fathy, A.; El-Kady, O.A. Effect of Al2O3 addition on hardness and wear behavior of Cu–Al2O3 electro-less coated Ag nanocomposite. J. Mater. Res. Technol. 2020, 9, 5024–5033. [Google Scholar] [CrossRef]
  6. Sadoun, A.M.; Fathy, A.; Abu-Oqail, A.; Elmetwaly, H.T.; Wagih, A. Structural, mechanical and tribological properties of Cu–ZrO2/GNPs hybrid nanocomposites. Ceram. Int. 2020, 46, 7586–7594. [Google Scholar] [CrossRef]
  7. Fang, Z.Z.; Paramore, J.D.; Sun, P.; Chandran, K.S.R.; Zhang, Y.; Xia, Y.; Cao, F.; Koopman, M.; Free, M. Powder metallurgy of titanium – past, present, and future. Int. Mater. Rev. 2018, 63, 407–459. [Google Scholar] [CrossRef]
  8. Cai, C.; Song, B.; Qiu, C.; Li, L.; Xue, P.; Wei, Q.; Zhou, J.; Nan, H.; Chen, H.; Shi, Y. Hot isostatic pressing of in-situ TiB/Ti-6Al-4V composites with novel reinforcement architecture, enhanced hardness and elevated tribological properties. J. Alloy. Compd. 2017, 710, 364–374. [Google Scholar] [CrossRef] [Green Version]
  9. Cai, C.; He, S.; Li, L.; Teng, Q.; Song, B.; Yan, C.; Wei, Q.; Shi, Y. In-situ TiB/Ti-6Al-4V composites with a tailored architecture produced by hot isostatic pressing: Microstructure evolution, enhanced tensile properties and strengthening mechanisms. Compos. Part B Eng. 2019, 164, 546–558. [Google Scholar] [CrossRef]
  10. Sedehi, S.M.R.; Khosravi, M.; Yaghoubinezhad, Y. Mechanical properties and microstructures of reduced graphene oxide reinforced titanium matrix composites produced by spark plasma sintering and simple shear extrusion. Ceram. Int. 2021, 47, 33180–33190. [Google Scholar] [CrossRef]
  11. Singh, N.; Ummethala, R.; Karamched, P.S.; Sokkalingam, R.; Gopal, V.; Manivasagam, G.; Prashanth, K.G. Spark plasma sintering of Ti6Al4V metal matrix composites: Microstructure, mechanical and corrosion properties. J. Alloy. Compd. 2021, 865, 158875. [Google Scholar] [CrossRef]
  12. Vasanthakumar, K.; Ghosh, S.; Koundinya, N.; Ramaprabhu, S.; Bakshi, S.R. Synthesis and mechanical properties of TiCx and Ti(C,N) reinforced Titanium matrix in situ composites by reactive spark plasma sintering. Mater. Sci. Eng. A 2019, 759, 30–39. [Google Scholar] [CrossRef]
  13. Savvakin, D.H.; Humenyak, M.M.; Matviichuk, M.V.; Molyar, O.H. Role of Hydrogen in the Process of Sintering of Titanium Powders. Mater. Sci. 2012, 47, 651–661. [Google Scholar] [CrossRef]
  14. Ivasishin, O.M.; Markovsky, P.E.; Savvakin, D.G.; Stasiuk, O.O.; Rad, M.N.; Prikhodko, S.V. Multi-layered structures of Ti-6Al-4V alloy and TiC and TiB composites on its base fabricated using blended elemental powder metallurgy. J. Mater. Process. Technol. 2019, 269, 172–181. [Google Scholar] [CrossRef]
  15. Ivasishin, O.; Bagliuk, G.; Stasiuk, O.; Savvakin, D.G. The Peculiarities of Structure Formation upon Sintering of TiH2+TiB2 Powder Blends. Phys. Chem. Solid State 2017, 18, 15–20. [Google Scholar] [CrossRef] [Green Version]
  16. Selvakumar, M.; Chandrasekar, P.; Ravisankar, B.; Balaraju, J.N.; Mohanraj, M. Mechanical Properties of Titanium–Titanium Boride Composites through Nanoindentation and Ultrasonic Techniques—An Evaluation Perspective. Powder Metall. Met. Ceram. 2015, 53, 557–565. [Google Scholar] [CrossRef]
  17. Song, Y.; Dong, S.; Stasiuk, O.; Savvakin, D.; Ivasishin, O. Synthesis of Ti/TiB Composites via Hydrogen-Assisted Blended Elemental Powder Metallurgy. Front. Mater. 2020, 364. [Google Scholar] [CrossRef]
  18. Schumann, E.; Silvain, J.-F.; Bobet, J.-L.; Bardet, M.; Lu, Y.; Kotousov, A.; Lamirand-Majimel, M. The effects of ball milling and the addition of blended elemental aluminium on the densification of TiH2 power. Mater. Chem. Phys. 2016, 173, 106–116. [Google Scholar] [CrossRef]
  19. Fouzia, H.; Mamoun, F.; Naouel, H.; Linda, A.; Goussem, M.; Said, M.; Mohammed, A.S.; Alex, M.; Iost, A.; Weiß, S.; et al. The effect of milling time on the microstructure and mechanical properties of Ti-6Al-4Fe alloys. Mater. Today Commun. 2021, 27, 102428. [Google Scholar] [CrossRef]
  20. Panek, J.; Karolus, M. Structural studies on Ti–Cu alloy obtained by high-energy ball milling. Mater. Sci. Technol. 2020, 36, 978–981. [Google Scholar] [CrossRef]
  21. Ivasishin, O.M.; Anokhin, V.M.; Demidik, A.N.; Savvakin, D.G. Cost-Effective Blended Elemental Powder Metallurgy of Titanium Alloys for Transportation Application. Key Eng. Mater. 2000, 188, 55–62. [Google Scholar] [CrossRef]
  22. Dong, S.; Ma, G.; Lei, P.; Cheng, T.; Savvakin, D.; Ivasishin, O. Comparative study on the densification process of different titanium powders. Adv. Powder Technol. 2021, 32, 2300–2310. [Google Scholar] [CrossRef]
  23. Dong, S.; Wang, B.; Song, Y.; Ma, G.; Xu, H.; Savvakin, D.; Ivasishin, O. Comparative Study on Cold Compaction Behavior of TiH2 Powder and HDH-Ti Powder. Adv. Mater. Sci. Eng. 2021, 2021, 9999541. [Google Scholar] [CrossRef]
  24. Ivasishin, O.; Moxson, V. 8-Low-cost titanium hydride powder metallurgy. In Titanium Powder Metallurgy; Qian, M., Froes, F.H.S., Eds.; Butterworth-Heinemann: Oxford, UK, 2015; pp. 117–148. ISBN 978-0-12-800054-0. [Google Scholar]
Figure 1. SEM-SE images of the starting powders: (a) HDH-Ti, (b) TiH2, (c) TiB2, (d) Al-V master alloy.
Figure 1. SEM-SE images of the starting powders: (a) HDH-Ti, (b) TiH2, (c) TiB2, (d) Al-V master alloy.
Materials 15 01049 g001
Figure 2. X-ray diffraction pattern of powder blends: (A) sample 1, (B) sample 2, (C) sample 3; and sintered composites: (D) sample 1, (E) sample 2, (F) sample 3.
Figure 2. X-ray diffraction pattern of powder blends: (A) sample 1, (B) sample 2, (C) sample 3; and sintered composites: (D) sample 1, (E) sample 2, (F) sample 3.
Materials 15 01049 g002
Figure 3. SEM-SE images of milled HDH-Ti+TiB2 powder blend at different magnifications. Blend milled for 4 h is presented as an example to show (a) typical morphology of particles and (b) TiB2 particles embedded into surface of Ti particle.
Figure 3. SEM-SE images of milled HDH-Ti+TiB2 powder blend at different magnifications. Blend milled for 4 h is presented as an example to show (a) typical morphology of particles and (b) TiB2 particles embedded into surface of Ti particle.
Materials 15 01049 g003
Figure 4. Microstructures (SEM-BSE) of composites produced with different preliminary milling times of HDH Ti+TiB2 powders: (a) 2 h, sample 1, (b) 4 h, sample 2, (c) 6 h, sample 3.
Figure 4. Microstructures (SEM-BSE) of composites produced with different preliminary milling times of HDH Ti+TiB2 powders: (a) 2 h, sample 1, (b) 4 h, sample 2, (c) 6 h, sample 3.
Materials 15 01049 g004
Figure 5. Microstructures of composites (SEM-BSE) produced with different HDH Ti-TiH2 proportions: (a) sample 4 (0:4), (b) sample 5 (1:3), (c) sample 6 (3:1), (d) sample 7 (4:0).
Figure 5. Microstructures of composites (SEM-BSE) produced with different HDH Ti-TiH2 proportions: (a) sample 4 (0:4), (b) sample 5 (1:3), (c) sample 6 (3:1), (d) sample 7 (4:0).
Materials 15 01049 g005
Figure 6. Engineering compressive strength–strain curves of composites produced with different HDH-Ti to TiH2 proportions.
Figure 6. Engineering compressive strength–strain curves of composites produced with different HDH-Ti to TiH2 proportions.
Materials 15 01049 g006
Table 1. Contents of oxygen, nitrogen and hydrogen in starting powders.
Table 1. Contents of oxygen, nitrogen and hydrogen in starting powders.
PowderOxygen (wt%)Nitrogen (wt%)Hydrogen (wt%)
TiH20.1950.533~3.5
HDH Ti0.1250.01340.00123
Master alloy0.2170.190.00213
TiB20.8550.5330.0089
Table 2. Variation of processing parameters used for manufacturing of Ti6Al4V-5 vol%TiB composites.
Table 2. Variation of processing parameters used for manufacturing of Ti6Al4V-5 vol%TiB composites.
Powder Blend (Sample) No.Duration of Pre-Milling (h)HDH-Ti to TiH2 Ratio (Mass Fractions)Sintering Regime
121:11250 °C
4 h
241:1
361:1
440:4
541:3
643:1
744:0
Table 3. Microstructural and hardness characteristics as well as oxygen content of sintered Ti6Al4V-5%TiB composites.
Table 3. Microstructural and hardness characteristics as well as oxygen content of sintered Ti6Al4V-5%TiB composites.
Blend No.Average TiB Length
(μm)
Hardness (HV)Porosity (%)Oxygen (wt%)
128.7307.5 ± 7.52.3 ± 0.10.337
221.4350 ± 100.6 ± 0.030.374
318.9372.5 ± 12.50.5 ± 0.030.43
422.7250 ± 104.3 ± 0.150.313
521.2335 ± 101.4 ± 0.050.356
622.4340 ± 101.1 ± 0.040.392
723.5355 ± 51.2 ± 0.050.455
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Song, Y.; Qiu, F.; Savvakin, D.; Xu, X.; Stasiuk, O.; Ivasishin, O.; Cheng, T. In Situ Ti6Al4V/TiB Composites Prepared by Hydrogen-Assisted Sintering of Blends Containing TiH2 and Ball-Milled Ti+TiB2 Powders. Materials 2022, 15, 1049. https://doi.org/10.3390/ma15031049

AMA Style

Song Y, Qiu F, Savvakin D, Xu X, Stasiuk O, Ivasishin O, Cheng T. In Situ Ti6Al4V/TiB Composites Prepared by Hydrogen-Assisted Sintering of Blends Containing TiH2 and Ball-Milled Ti+TiB2 Powders. Materials. 2022; 15(3):1049. https://doi.org/10.3390/ma15031049

Chicago/Turabian Style

Song, Yuchao, Fucheng Qiu, Dmytro Savvakin, Xiaofeng Xu, Oleksandr Stasiuk, Orest Ivasishin, and Tuo Cheng. 2022. "In Situ Ti6Al4V/TiB Composites Prepared by Hydrogen-Assisted Sintering of Blends Containing TiH2 and Ball-Milled Ti+TiB2 Powders" Materials 15, no. 3: 1049. https://doi.org/10.3390/ma15031049

APA Style

Song, Y., Qiu, F., Savvakin, D., Xu, X., Stasiuk, O., Ivasishin, O., & Cheng, T. (2022). In Situ Ti6Al4V/TiB Composites Prepared by Hydrogen-Assisted Sintering of Blends Containing TiH2 and Ball-Milled Ti+TiB2 Powders. Materials, 15(3), 1049. https://doi.org/10.3390/ma15031049

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop