Next Article in Journal
Metallurgical Coke Production with Biomass Additives: Study of Biocoke Properties for Blast Furnace and Submerged Arc Furnace Purposes
Next Article in Special Issue
Recycling Unused Midazolam Drug as Efficient Corrosion Inhibitor for Copper in Nitric Acid Solution
Previous Article in Journal
Increasing Impact Strength of a Short Glass Fiber Compression Molded BMC by Shortening Fibers without Change in Equipment
Previous Article in Special Issue
Analysis of Multiphase Flow and Heat and Mass Transfer for Ammonium Chloride Crystallization of the High-Pressure Heat Exchanger in Hydrogenation Unit
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Synthesis of Novel Nano-Sulfonamide Metal-Based Corrosion Inhibitor Surfactants

by
Manal M. Khowdiary
1,2,*,
Nahla A. Taha
3,*,
Nashwa M. Saleh
4 and
Ahmed A. Elhenawy
5,6
1
Chemistry Department, Faculty of Applied Science, Umm Al-Qura University Branch El Lieth, Makkah al-Mukarramah 24382, Saudi Arabia
2
Applied Surfactant Laboratory, Egyptian Petroleum Research Institute, Cairo 11727, Egypt
3
Modeling and Simulation Research Department, Advanced Technology and New Materials Research Institute, City of Scientific Research and Technological Applications (SRTA-CITY), New Borg El-Arab City 21934, Egypt
4
Egypt Department of Chemistry, Faculty of Science, Al-Azhar University (Girls Branch), Youssef Abbas Str., Cairo 11651, Egypt
5
Department of Chemistry, Faculty of Science and Arts in Al-Mukhwah, Al-Baha University, Al Bahah 65511, Saudi Arabia
6
Chemistry Department, Al-Azhar University, Cairo 11651, Egypt
*
Authors to whom correspondence should be addressed.
Materials 2022, 15(3), 1146; https://doi.org/10.3390/ma15031146
Submission received: 19 November 2021 / Revised: 13 January 2022 / Accepted: 25 January 2022 / Published: 1 February 2022
(This article belongs to the Special Issue Research of Corrosion Behavior of Metallic Materials)

Abstract

:
The synthesis of novel corrosion inhibitors and biocide metal complex nanoparticle surfactants was achieved through the reaction of sulfonamide with selenious acid to produce a quaternary ammonium salt. Platinum and cobalt surfactants were then formed by complexing the first products with platinum (II) or cobalt (II) ions. The surface properties of these surfactants were then investigated, and the free energy of form micelles (ΔGomic) and adsorption (ΔGoads) was determined. The obtained cationic compounds were evaluated as corrosion inhibitors for carbon steel dissolution in 1N HCl medium. The results of gravimetric and electrochemical measurements showed that the obtained inhibitors were excellent corrosion inhibitors. The anti-sulfate-reducing bacteria activity known to cause corrosion of oil pipes was obtained by the inhibition zone diameter method for the prepared compounds, which were measured against sulfate-reducing bacteria. FTIR spectra, elemental analysis, H1 NMR spectrum, and 13C labeling were performed to ensure the purity of the prepared compounds.

1. Introduction

Worldwide, corrosion is one of the greatest problems that educational and industrial divisions must solve because it has a negative effect on the economy of developing and developed countries [1,2]. Corrosion, which results from the presence of a carbon steel in acidic medium, can be reduced by adding corrosion inhibitors in modest amounts [3,4,5,6,7,8,9]. The majority of commercially available acid inhibitors are organic molecules containing heteroatoms, such as sulfur [10], oxygen [11], nitrogen [12,13], and phosphorous. Many heterocyclic compounds containing nitrogen atoms have been found to be excellent inhibitors of steel corrosion in acidic environments [14,15,16,17,18]. Quaternary ammonium salt (QAS) is a famous product utilized in numerous applications of corrosion inhibition of oil pipes. Most of the world’s QAS production involves cationic surfactants, which are widely used on different types of industrial oil protection equipment as well as on closed cooling systems. Synthesis and mass production of these inhibitors have been the primary focus of recent research in science and chemical engineering [19,20,21,22,23]. Biocides are chemical compounds that are capable of preventing or suppressing the growth of bacteria and fungi in different environments. The defeating strategy against lethal microorganisms, especially in the industrial field, involves the use of environmental biocides to protect the environment and living organisms [24,25]. These compounds have other important applications, such as cutting fluids, which are used in various machining operations. Water-miscible cutting fluid has been a recent trend towards water-based fluids. It has the advantage of low toxicity and excellent cooling capacity, and it overcomes problems associated with mineral oil-based products, such as unpleasant odor, oil mist formation, and fumes at high temperatures. However, for water-based cutting fluids to offer a practical alternative, they must possess good rust-inhibiting, anti-wear, and anti-microbial activity [26].
Obviously, in strongly acidic media, most organic inhibitors undergo protonation and exist in their cationic (positive) forms. Conversely, metallic surfaces become negatively charged in acidic solutions due to the adsorption of anionic counter ions of acids (e.g., Cl, SO42−, −NO3−) [27]. Thus, organic inhibitors initially engage with metallic surfaces through electrostatic attraction forces (i.e., physisorption), and then interact with metallic surfaces utilizing non-binding ions and electrons to form coordination bonds (i.e., chemisorption) [28]. Quaternary ammonium salts have been shown to be exceedingly cost-effective and are frequently employed in the H2SO4 medium to prevent mild steel corrosion. The efficiency of N-alkyl quaternary ammonium compounds with increasing alkyl chain lengths in reducing acid corrosion of mild steel has been demonstrated [29]. In acid solution, bis quaternary ammonium compounds have also been investigated as corrosion inhibitors [30]. Adsorption is a process in which the inhibitor is absorbed into the body. Adsorption of inhibitors with alkyne moieties causes polymerization of the inhibitors on the metal surface, which results in the creation of a journal pre-proof protective film (coating) and hence, inhibitory effects [31]. Hydrophobic alkyl chains have been shown to boost inhibitory efficiency [32]. Some of these include pyridines, pyrimidines, imidazoles, triazoles, quinolines, naphthyridines, benzothiazoles, benzimidazoles, benzotriazoles, and other similar groups of compounds. The presence of heteroatoms (N, S, O, etc.), bonds, and an aromatic ring structure in these molecules allow them to coordinate with metallic substrates efficiently [33,34]. The purpose of this study was to produce novel compounds that are not hazardous to humans, have a low environmental impact, are biodegradable, and have high inhibition efficiency at low costs. This novel product also may be characterized as a multifunctional material that acts as a biocide, corrosion inhibitor, and emulsifying agent in oil production systems.

2. Materials and Methods

All chemicals were produced from Sigma-Aldrich, St. Louis, MO, USA such as selenious acid (H2SeO3); sulfonamide; ethyl alcohol (C2H5OH); diethyl ether (C2H5O); PtCl2; CoCl4; petroleum ether; cyclodextrin oligosaccharide, carbon steel strips of following composition (by weight, wt.%): C = 0.07, Mn = 0.19, P = 0.02, Si = 0.03, Cr = 0.05, Al = 0.02, Cu = 0.12 and balance Fe.

2.1. Preparation of Test Samples

2.1.1. Synthesis of Sulfonamide Hydrogen Selenites IIa

To carry out the synthesis process, stoichiometric amounts of selenious acid were mixed with sulfonamide in diethyl ether at 25 °C with vigorous shaking until precipitation was complete. Then, products were filtered and washed with acetone and were recrystallized by petroleum ether [35]. The products were designated as IIa and have the general formula:
RNH3 HSeO3
where R = sulfonamide

2.1.2. Synthesis of Metal Complexes

(a)
Synthesis of cobalt and platinum hydrogen selenite dehydrate [35].
PtCl2·2H2O + Na2CO3 → PtCO3·2H2O + 2NaCl
CoCl2·2H2O + Na2CO3 → CoCO3·2H2O + 2NaCl
PtCO3·2H2O + 2H2SeO3 → Pt(HSeO3)2 +2H2O
CoCO3·2H2O + 2H2SeO3 → Co(HSeO3)2 + 2H2O
(b)
Synthesis of platinum and cobalt ammonium hydrogen selenite complexes IIb,c.
Platinum or cobaltsulfonammonium hydrogen selenite complexes were prepared by refluxing two moles of sulfonammonium hydrogen selenites (IIa) with one mole of platinum or cobalt hydrogen selenite in ethyl alcohol for two hours. The products were designated as (IIb,c), as shown in Figure 1.
2RNH3 (HSeO3)2 + M (HSeO3)4 → (RNH3)2M(HSeO3)4
where
M = Pt or Co  R = sulfon
Compound IIb, Yield, 72%; m.p. 172–174 _C; IR, (KBr, cm−1): disappear of NH2 according to form quaternary salt, 3053 (CH arom.), 1370, 1155 (SO2). 1H-NMR (DMSO-d6) δ: 4.6 (s, 1H, NH, exchangeable with D2O), 7.3–8.0 (m, 10H, Ar-H + SO2NH2, exchangeable with D2O). MS m/z (%): 1056 (57.77), 172 (100). Anal. Calcd. For C12H22N4O16S2PtSe4 (1056.68): C, 13.68; H, 2.11; N, 5.32; O, 24.30; Pt, 18.52; S, 6.09; Se, 29.98. Found: C, 13.56; H, 2.08; N, 5.29; O, 24.24; Pt, 18.42; S, 5.99; Se, 29.78.
Compound IIc, Yield, 82%; m.p. 210-212 _C; IR, (KBr, cm−1): disappear of NH2 according to form quaternary salt, 3052 (CH arom.), 1373, 1156 (SO2). 1H-NMR (DMSO-d6) δ: 4.5 (s, 1H, NH, exchangeable with D2O), 7.6–8.3 (m, 10H, Ar-H + SO2NH2, exchangeable with D2O). MS m/z (%): 920 (37.16), 172 (100). Anal. Calcd. For C12H22N4O16S2PtSe4 (920.65): C, 15.71; H, 2.42; Co, 6.43; N, 6.11; O, 27.91; S, 6.99; Se, 34.43. Found: C, 15.69; H, 2.32; Co, 6.39; N, 6.09; O, 27.83; S, 6.86; Se, 34.37.

2.1.3. General Formula for the Metal Complexes

Metal complex prepared using either platinum or cobalt ([RNH3] + 2Pt[(HSeO3)−4], [RNH3] + 2Co[(HSeO3)]4 ) may be formulated as expected with the chemical structure shown in (Figure 2)

2.1.4. Green Synthesis with Solid State Reaction in Ball Mill for Complex Nanoparticles

The method of synthesizing organic compounds using a ball mill as a reactor is an environmentally safe method for using green chemistry. By comparing this technique with normal solution methods, it presents many advantages, such as reducing the number of solvents used, thereby reducing the number of volatile compounds. Heavy mixing in the solid state helps disintegration and mobility for rapid friction among molecules in a short amount of time. For non-polar and polar solvents, mixing problems are reduced. The energy used to complete the reaction is reduced due to the optimum use of energy in the reaction mixture. The nano-sized particles of Co and Pt complexes were achieved by mixing them very well with cyclodextrin oligosaccharides using ceramic mortar. Finally, both were ground using a ball mill model PM 200 (TMAXC-Fujian, China) at 300 rpm for 3 h.

2.1.5. Evaluation of Anti-Sulfate-Reducing Bacteria Activity

The inhibition zone diameter (Iz D) Method: a filter paper sterilized disc saturated with a measured quantity of the sample was placed on a plate containing a solid bacterial medium (nutrient agar broth) that had been heavily seeded with the spore suspension of the tested bacteria. After incubation, the diameter of the clear zone of inhibition surrounding the sample was taken as a measure of the inhibitory power of the sample against the particular test organism. All sulfate-reducing bacteria were provided by a culture collection of the Regional Center for Mycology and Biotechnology (RCMB), Al-Azhar University, Cairo, Egypt.

2.2. Corrosion Inhibition Measurements

2.2.1. Weight Loss Measurements

The carbon steel specimens have a composition of (wt %): 0.21 C, 0.035 Si, 0.25 Mn, 0.082 P, and the remainder is Fe. The carbon steel sheets of 2.5 cm × 2.0 cm × 0.6 cm were abraded with emery papers (grades 320, 500, 800 and 1200) and then washed with distilled water and acetone. After weighing accurately, the specimens were immersed in a 250 mL beaker containing 200 mL of 0.5 M hydrochloric acid alone or with 50, 100, 200, or 400 ppm by weight of the inhibitors used at 25 °C. After different immersion time intervals of 1, 3, 6, and 24 h, the specimens were taken out, washed, dried, and weighed accurately. The corrosion rate (K) and the inhibition efficiency (η %) were calculated using the following equations [36].
K = (W/St)
ηw % = [{Wcorr − Wcorr(inh)}/Wcorr] × 100
where W is the average weight loss of three parallel carbon steel sheets (one specimen in each beaker), S is the total area of the steel specimen, and t is immersion time. Wcorr and Wcorr(inh) are the corrosion rates obtained in the absence and the presence of inhibitors, respectively.

2.2.2. Polarization Measurements

Electrochemical measurements are made in the traditional cylindrical cells made of Pyrex glass with a triple electrode, the working electrode (WE) in the form of steel rods embedded with polytetrafluoroethylene (PTFE; the Free Zone of the electrode that was exposed to the analysis of the electrical 0.7 cm2) and saturated calomel electrode (SCE), a platinum electrode used as auxiliary, and a standard electrode, respectively. Polarization measurements were carried out using a potentiostat (Wenking, Wuhan, China). The working electrode was immersed in the test solution for 45 min to reach the open circuit potential. (The carbon steel used in the polarization measurements was identical to that used in the weight loss measurements.) Next, the working electrode was polarized in both cathodic and anodic directions. In terms of accuracy of the calculated slopes, the values were compared with the obtained data from the software calculations accompanied with a potentiostat (Wenking, Wuhan, China), and the accuracy was 4%. The values of corrosion current density (ICorr) were calculated via extrapolation of the straight part of the Tafel lines. A standard ASTM glass electrochemical cell was used, and the platinum electrode was used as an auxiliary electrode. The potential increased with a speed of 2 mV min−1, starting from −200 mV to +200 mV with respect to the open circuit potential (OCP) versus corrosion potential (ECorr) [36].

2.2.3. Scanning Electron Microscopy (SEM)

After dipping carbon steel samples in acidic solution, corrosion of the samples was tested with different concentrations of the corrosion inhibitor products to investigate the optimal concentration of each inhibitor at which the corrosion decreased. Exposing the samples for SEM also directly aided in studying the surface’s morphology.

3. Results and Discussion

3.1. Surface Properties of the Prepared Cationic Surfactants

As shown in Table 1 and Figure 3, after complexing ammonium hydrogen selenite with Co or Pt ions, a high depression in CMC, Ycmc, Amin value was observed for compounds designated as IIa, IIb and IIc compared to those of the complex designated as IIa. This may be because metal complexes have specific properties in water. The complexes in the solutions aggregate as units, which can increase the volume due to repulsion between the hydrophobic chain of the complexes and water molecules that can occur.
An increase in Pc20, ΠCMC, and Γmax value was observed for compounds designated as IIb and IIc in comparison to the complex designated as IIa. This may be attributed to the double chain of hydrocarbon groups in metal complexes, which by its role, increases the hydrophobicity, thereby causing an increase in the concentration at the interface (maximum surface excess Γmax). Froing of the great number of molecules at the interface leads to an increase in the effectiveness of ΠCMC and a greater reduction in surface tension at critical micelle concentration [37]. All the result values of ΔGads and ΔGmic were negative, which is considered evidence for carrying them out directly without increasing the temperature of the reaction system.

3.2. Antibacterial Activity of the Prepared Surfactants against Sulfate-Reducing Bacteria

Corrosion Inhibitor Activity for Oil Pipes

Sulfate-reducing bacteria (SRB) are considered reducers of sulfate, and their growth and reproduction cause oil pipe and equipment corrosion. This can lead to the loss of economy, and cause environmental, health, and safety hazards. Stabilized mixed culture accumulates with sulfate reducing bacteria. In many industrial sectors such as the oil and gas industry, it is important to minimize the evolution of hydrogen sulfide gas which can result from SRB activity. The results of the synthesized cationic surfactants against sulfur-reducing bacteria are recorded in Table 2.
As shown from Table 2, the novel products have high antibiological activity against SRB, while this activity also increased as we notice from the table. When products form complexes that have two hydrocarbon groups, hydrophobicity adsorption at the bacterial membrane increases. The protein and lipid molecules of the complex mobilize with the hydrocarbons of the inhibitor and the membrane breaks down, inhibiting the growth of DNA and thus no reproduction. Platinum complexes produced the best results, possibly because platinum is an oxidizing chemical agent that acts as a reduction inhibitor, reducing sulfide generation and slowing anaerobic growth (SRB). The specific activity of the tested bacteria was closely related to the rate of H2S generation and the generation time was inversely proportional to these activities. The rate of bacterial resistance to metal ions was directly proportional to the rate of microbiologically induced corrosion (MIC) of carbon steel.

3.3. Results of Weight Loss (Gravimeteric) Method and Effect of Inhibitor Concentration

Table 3 and Table 4 describe the variations in corrosion rate (K values) of the dissolution reaction of carbon steel in 1 M HCl solution in the presence of IIb and IIc inhibitors at different concentrations, respectively. It is obvious that a gradual increase in inhibitor concentrations from 1 × 10−4 to 1 × 10−2 M by weight reduces the K values considerably. At 1 × 10−4 M by weight of the IIb and IIc inhibitors, the K values of carbon steel were high. In contrast, increasing the inhibitor concentration to 1 × 10−2 M by weight decreases K to the lowest value. This is due to an increase in the number of adsorbed inhibitor molecules on the metal surface caused by an increase in the inhibitor concentration in the medium. In turn, this improves surface protection and slows the metal dissolution reaction. The number of inhibitor molecules adsorbed on the metal surface increases as the inhibitor concentration increases. As a result, this increases the surface area covered by inhibitor molecules and consequently decreases the dissolution of metal due to the reaction of metal by corrosive ions in the medium [37].

3.4. Electrochemical Evaluation

Potentiodynamic Polarization Spectroscopy

Cathodic and anodic current for carbon steel corrosion in 1 M HCl in the presence of 1 × 10−2 to 1 × 10−4 M by weight of the synthesized inhibitors IIb, IIc at 25 °C. Figure 4 represents the relation for (IIb) where (βc, βa): the electrochemical polarization parameter of cathodic and anodic Tafel slopes; (Icorr): corrosion current density; (Ecorr): potential of corrosion; (η): inhibition efficiency obtained from this figure were listed in Table 5. The corrosion currents decreased in the presence of the inhibitors as indicated by low values, such as 0.06, 0.04, 0.02, and 0.24 mA cm−2 for 1 × 10−4 to 1 × 10−2 M by weight of II b respectively. Surface coverage (θ) of the carbon steel by the inhibitor molecules was determined by using the values of the corrosion currents in the following equation [38]:
θ = (icorr(uninh) − Icorr(inh))/(Icorr(uninh))
where Icorr (uninh) is the corrosion current density with the presence of different inhibitors and Icorr(inh) is the corrosion current density in the absence of the different inhibitors.
Corrosion inhibition efficiencies can be calculated from the previous values with different concentrations of the inhibitors using the following equation [39]:
η% =(Icorr(uninh) − Icorr(inh))/(Icorr(uninh)) × 100
As shown in Table 5, at 1 × 10−2 M by weight, the value of icorr in the case of IIc (0.020 mA cm−2) is smaller than that of IIb, while accordingly, the values of inhibition efficiencies in the presence of IIc (94.68) is greater than that of IIb (83.01%). From the polarization curves displayed in Figure 4, the decrease in the two reactions at the cathode and anode occurs in the absence of the synthesized corrosion inhibitors but not in the presence of them. Additionally, increasing the concentration from 1 × 10−4 M to 1 × 10−2 M by weight increases inhibition. It may be that the presence of inhibitors in higher concentrations reduced the anodic dissolution and suppressed the reduction of hydrogen ions [40,41]. As shown in Figure 4, by increasing the concentration of the synthesized product, the cathodic current densities sharply decreased, which may be due to the formation of a covered separation film which developed from a single layer of the synthesized product onto the cathodic sites of the carbon steel [42]. The corrosion current densities increased slowly at the start of anodic polarization, and the anodic polarization was mostly facilitated by the positive shift in polarization potential. This indicates that the adsorption rate of the inhibitor molecules on the carbon steel surface is greater than their desorption rate and that the adsorption process controls the anodic reaction (as in Figure 5). The polarization behavior was comparable, implying that the inhibitor molecules are fully adsorbed from the solution to the carbon steel surface and that increasing the concentration increases their inhibition action [43]. When the inhibitor concentration increases, corrosion decreases. With increasing inhibitor concentrations, the protective coating adsorbed onto the metal surface tends to be more complete. This is supported by the increase in corrosion current densities and the increase in η%. When the corrosion potential shifts to values greater than 85 mV (compared to the corrosion potential without inhibitors), the inhibitors are categorized as cathodic or anodic [44]. However, for all the inhibitors tested, the Ecorr displacement is less than 85 mV. As a result, these inhibitors are known as mixed-type inhibitors [45,46].

3.5. Docking Study

Docking investigations based on potent–protein interactions are used to explain the biological results. Figure 6 shows all of the docking computations. Protein data library was used to obtain the X-ray crystal structures of the following bacterial strains: A. fumigatus (ID [47]; 5HWC), G. Candidum (ID [48]; 4ZZt), S. Pneumoniae (ID [49]; 5LJI), and E. Coli (ID [50]; 3t88), respectively. The following are the essential backbone amino acid residues retrieved via X-rays analysis: Tyr27, Asp38, Arg55, Ile57, and Tyr83 for 5HWC; Arg339, Arg251, Glu212, and Asp259 for 4ZZW; Gly 60, Glu97, Cys99, Asp92, Thr15, Asn14, Ser90, and Thr58 for 5LJI; Tyr57, Asn42, Thr203, Arg188, and Glu213 for 3t88. These amino acid residues hindered microbial action through chelating with reference inhibitors. Ag/TNTs-P400 was the most effective at docking into kinase receptors. MOE-scoring for the most stable docking model was used to evaluate the binding affinity of complexes (inhibitor-kinase) (Figure 6). With an MMFF94 force field, the complexes were energy-minimized until the gradient for the restricted convex was minimized to 0.05 kcal/mol. IIb was the most effective at docking onto kinase receptors. MOE-scoring was used to identify the most stable docking model used to evaluate the binding affinity of complexes (inhibitor-kinase) (Figure 6). For all kinases, the studied sample was successfully docked onto active sites. In Figure 6, the hydrogen bond interactions between the ligand and the receptor were discovered in the construction of active nanocomposites. The hydrophobic cation-π interactions at a distance >6 Å are not shown in Figure 7. In the absence of H-bond interactions, IIa docked onto the active sites 5HWC, 4ZZt, 5LJI, and 3t88, which gave insignificant binding energies (Figure 7). The sample has the greatest binding score (G =~ −4 Kcal/mol) against the 4ZZt active site.
The kinase reset inhibition potency assumed the following pattern: 5LJI>3t88 >5HWC, with promising binding score values (Figure 7). Amino acid residues interact with samples by forming significant E.H.B of H-bonds with energies ranging from ~ −8 to −5 kcal/mol. Against the 4ZZt binding pocket, the studied materials had the highest stabilization energy (Eint = −8.267 kcal/mol). On the other hand, those found at the 3t88 active site had the lowest stabilization energy (Eint = −2.140 kcal/mol). In comparison to 5LJI binding pockets, 5HWC binding pockets yielded less stabilization energy (Figure 7).

4. Conclusions

This work aimed to synthesize novel antibiotic quaternary ammonium salt nano-surfactants based on sulfonamide with selenious acid and complexed with platinum and cobalt surfactant. We used FTIR spectra, elemental analysis, H1 NMR spectrum, and 13C labeling to investigate the surface behaviors of these surfactants as free energy to form micelles (ΔGomic) and adsorption (ΔGoads). In 1N HCl media, we assessed the generated cationic compounds as corrosion inhibitors for carbon steel. Gravimetric and electrochemical studies revealed that the studied inhibitors are excellent corrosion inhibitors. The anti-sulfate-reducing bacteria activity, which causes the corrosion of oil pipes, was obtained by the inhibition zone diameter method for the prepared compounds, which measured against sulfate-reducing bacteria. Particle size scaled into the nano-range, which required investigation via transmitted electron microscope (TEM). Finally, the DFT using B3LYP and the 6-311G* correlation function was applied for the investigated probes. DFT and MEPs were also used to identify the interaction compound’s behavior over heavy metal for water formation.

Author Contributions

M.M.K. participated in conceptualization, data interpretation, manuscript writing, and manuscript review, revision, and refinement; N.A.T. participated in validation, original draft, writing, interpreting, and reviewing the manuscript; N.M.S. participated in methodology, performed experiments work; A.A.E. participated in data interpretation, manuscript writing, and manuscript review in data analyses. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The data presented in this study are contained within the article.

Acknowledgments

The authors would like to thank the Deanship of Scientific Research at Umm Al-Qura University for the continuous support. This work was supported by the Deanship of Scientific Research at Umm Al-Qura University to Manal Khowdiary (Grant Code: 19-SCI-1-03-0015).

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Verma, C.; Haque, J.; Quraishi, M.A.; Ebenso, E.E. Aqueous phase environmental friendly organic corrosion inhibitors derived from one step multicomponent reactions: A review. J. Mol. Liq. 2018, 275, 18–40. [Google Scholar] [CrossRef]
  2. Verma, C.; Ebenso, E.E.; Quraishi, M. Ionic liquids as green and sustainable corrosion inhibitors for metals and alloys: An overview. J. Mol. Liq. 2017, 233, 403–414. [Google Scholar] [CrossRef]
  3. Popova, A. Temperature effect on mild steel corrosion in acid media in presence of azoles. Corros. Sci. 2007, 49, 2144–2158. [Google Scholar] [CrossRef]
  4. Ahamad, I.; Quraishi, M.A. Bis-(benzimidazol-2-yl) disulphide: An efficient water soluble inhibitor for corrosion of mild steel in acid media. Corros. Sci. 2009, 51, 2006–2013. [Google Scholar] [CrossRef]
  5. Obot, I.B.; Obi-Egbedi, N.O. Adsorption properties and inhibition of mild steel corrosion in sulphuric acid solution by ketoconazole: Experimental and theoretical investigation. Corros. Sci. 2010, 52, 198–204. [Google Scholar] [CrossRef]
  6. Popova, A.; Sokolova, E.; Raicheva, S.; Christov, M. AC and DC study of the temperature effect on mild steel corrosion in acid media in the presence of benzimidazole derivatives. Corros. Sci. 2003, 45, 33–58. [Google Scholar] [CrossRef]
  7. Shukla, S.K.; Quraishi, M.A. 4-Substituted anilinomethyl propionate: New and efficient corrosion inhibitors for mild steel in hydrochloric acid solution. Corros. Sci. 2009, 51, 1990–1997. [Google Scholar] [CrossRef]
  8. Behpour, M.; Ghoreishi, S.M.; Soltani, N.; Salavati-Niasari, M.; Hamadanian, M.; Gandomi, A. Electrochemical and theoretical investigation on the corrosion inhibition of mild steel by thiosalicylaldehyde derivatives in hydrochloric acid solution. Corros. Sci. 2008, 50, 2172–2181. [Google Scholar] [CrossRef]
  9. Qiu, L.; Wu, Y.; Wang, Y.; Jiang, X. Synergistic effect between cationic gemini surfactant and chloride ion for the corrosion inhibition of steel in sulphuric acid. Corros. Sci. 2008, 50, 576–582. [Google Scholar] [CrossRef]
  10. Hosseini, S.M.A.; Azimi, A. The inhibition of mild steel corrosion in acidic medium by 1-methyl-3-pyridin-2-yl-thiourea. Corros. Sci. 2009, 51, 728–732. [Google Scholar] [CrossRef]
  11. Ali, S.A.; Saeed, M.T.; Rahman, S.U. The isoxazolidines: A new class of corrosion inhibitors of mild steel in acidic medium Corros. Sci. 2003, 45, 253. [Google Scholar] [CrossRef]
  12. Li, W.; Zhao, X.; Liu, F.; Hou, B. Investigation on inhibition behavior of S-triazole–trizaole derivatives in acidic solution. Corros. Sci. 2008, 50, 3261–3266. [Google Scholar] [CrossRef]
  13. Palomar-Pardavé, M.; Romero-Romo, M.; Herrera-Hernández, H.; Abreu-Quijano, M.A.; Likhanova, N.V.; Uruchurtu, J.; Juárez-García, J.M. Influence of the alkyl chain length of 2-amino-5-alkyl-1,3,4- thiadiazole compounds on the corrosion inhibition of steel immersed in sulfuric acid solutions. Corros. Sci. 2012, 54, 231–243. [Google Scholar] [CrossRef]
  14. Chetouani, A.; Hammouti, B.; Benhadda, T.; Daoudi, M. Inhibitive action of bipyrazolic type organic compounds towards corrosion of pure iron in acidic media. Appl. Surf. Sci. 2005, 249, 375–385. [Google Scholar] [CrossRef]
  15. Popova, A.; Christov, M.; Raicheva, S.; Sokolova, E. Adsorption and inhibitive properties of benzimidazole derivatives in acid mild steel corrosion. Corros. Sci. 2004, 46, 1333–1350. [Google Scholar] [CrossRef]
  16. Obot, I.B.; Obi-Egbedi, N.O.; Umoren, S.Z. The synergistic inhibitive effect and some quantum chemical parameters of 2,3-diaminonaphthalene and iodide ions on the hydrochloric acid corrosion of aluminium. Corros. Sci. 2009, 51, 276–282. [Google Scholar] [CrossRef]
  17. Herrag, L.; Hammouti, B.; Elkadiri, S.; Aouniti, A.; Jama, C.; Vezin, H.; Bentiss, F. Adsorption properties and inhibition of mild steel corrosion in hydrochloric solution by some newly synthesized diamine derivatives: Experimental and theoretical investigations. Corros. Sci. 2010, 52, 3042–3051. [Google Scholar] [CrossRef]
  18. Wang, X.; Yang, H.; Wang, F. Role of nitrite addition in chloride stress corrosion cracking of a super duplex stainless steel. Corros. Sci. 2011, 53, 113–121. [Google Scholar] [CrossRef]
  19. Negm, N.A.; Kandile, N.G.; Badr, E.A.; Mohammed, M.A. Gravimetric and electrochemical evaluation of environmentally friendly nonionic corrosion inhibitors for carbon steel in 1M HCl. Corros. Sci. 2012, 65, 94–103. [Google Scholar] [CrossRef]
  20. Gust, J. Application of infrared spectroscopy for investigation of rust phase component conversion by agents containing oak tannin and phosphoric acid. NACE 1991, 47, 453–457. [Google Scholar] [CrossRef]
  21. Jaen, J.A.; Saldana, G.; Hernandez, C. Characterization of reaction products of iron and aqueous plant extracts. Hyperfine Interact. 1999, 122, 139–145. [Google Scholar] [CrossRef]
  22. Rahim, A.A.; Rocca, E.; Steinmetz, J.; Kassim, M.J. Inhibitive action of mangrove tannins and phosphoric acid on pre-rusted steel via electrochemical methods. Corros. Sci. 2008, 50, 1546–1550. [Google Scholar] [CrossRef]
  23. Ostovari, A.; Hoseinieh, S.M.; Peikari, M.; Shadizadeh, S.R.; Hashemi, S.J. Corrosion inhibition of mild steel in 1M HCl solution by henna extract: A comparative study of the inhibition by henna and its constituents. Corros. Sci. 2009, 51, 1935–1944. [Google Scholar] [CrossRef]
  24. Saroja, N.; Shamala, T.R.; Tharanathan, R.N. Biodegradation of starch-g-polyacrylonitrile, a packaging material, by Bacillus cereus. Process Biochem. 2000, 36, 119–125. [Google Scholar] [CrossRef]
  25. Rezende, R.; Dias, J.; Ferraz, V.; Basic, J. Metabolism of benzonitrile by Cryptococcus sp. UFMG-Y28. J. Basic Microbiol. 2000, 40, 389–392. [Google Scholar] [CrossRef]
  26. Holmes, P.M. Factors Affecting the Selection of Cutting Fluids. Ind. Lubr. Tribol. 1971, 2, 47–55. [Google Scholar] [CrossRef]
  27. Kumar, R.; Chopra, R.; Singh, G. Electrochemical, morphological and theoretical insights of a new environmentally benign organic inhibitor for mild steel corrosion in acidic media. J. Mol. Liq. 2017, 241, 9–19. [Google Scholar] [CrossRef]
  28. Fouda, A.; Ismail, M.; EL-Elewady, G.; Abousalem, A. Evaluation of 4-amidinophenyl2, 2′-bithiophene and its aza-analogue as novel corrosion inhibitors for CS in acidic media: Experimental and theoretical study. J. Mol. Liq. 2017, 240, 372–388. [Google Scholar] [CrossRef]
  29. Haque, J.; Jafar Mazumder, M.A.; Quraishi, M.A. Pyrrolidine-based quaternary ammonium salts containing propargyl and hydrophobic C-12 and C-16 alkyl chains as corrosion inhibitors in aqueous acidic media. J. Mol. Liq. 2020, 320, 11473. [Google Scholar] [CrossRef]
  30. Huilong, W.; Jiashen, Z.; Jing, L. Inhibition of the corrosion of carbon steel in hydrochloric acid solution by bisquaternary ammonium salt. Anti-Corros. Method. M 2002, 49, 127–132. [Google Scholar] [CrossRef]
  31. Walker, M.L. Method and Composition for Acidizing Subterranean Formations. U.S. Patent 4498997, 12 February 1985. [Google Scholar]
  32. Ali, S.A.; El-Shareef, A.; Al-Ghamdi, R.; Saeed, M. The isoxazolidines: The effects of steric factor and hydrophobic chain length on the corrosion inhibition of mild steel in acidic medium. Corros. Sci. 2005, 47, 2659–2678. [Google Scholar] [CrossRef]
  33. Jing, C.; Wang, Z.; Gong, Y.; Huang, H.; Ma, Y.; Xie, H.; Li, H.; Zhang, S.; Gao, F. Photo and thermally stable branched corrosion inhibitors containing two benzotriazole groups for copper in 3.5 wt% sodium chloride solution. Corros. Sci. 2018, 138, 353–371. [Google Scholar] [CrossRef]
  34. Antonijević, M.M.; Milić, S.M.; Petrović, M.B. Films formed on copper surface in chloride media in the presence of azoles. Corros. Sci. 2009, 51, 1228–1237. [Google Scholar] [CrossRef]
  35. Badawi, A.M.; Mekawi, M.A.; Mohamed, M.Z.; Mohamed, A.S.; Khowdairy, M.M. Surface and Biological Activity of Organoammonium Hydrogen Selenite Surfactants. J. Surfactants Deterg. 2007, 10, 257–267. [Google Scholar] [CrossRef]
  36. Supuran, C.T.; Scozzafava, A. Carbonic anhydrases as targets for medicinal chemistry. Bioorg. Med. Chem. 2007, 15, 4336–4350. [Google Scholar] [CrossRef]
  37. Khowdiary, M.M.; El-Henawy, A.A.; Shawky, A.M.; Negm, N.A. Evaluation of cationic inhibitors derived from recycled polyethylene terephthalate wastes in protection of carbon steel against acidic corrosion in oil fields. J. Mol. Liq. 2020, 320, 114504. [Google Scholar] [CrossRef]
  38. Khowdiary, M.M.; El-Henawy, A.A.; Shawky, A.M.; Sameeh, M.Y.; Negm, N.A. Synthesis, characterization of silver nanoparticles-cationic quaternary ammonium polymers and evaluation as biocides against sulfate reducing bacteria. J. Mol. Liq. 2016, 12, 939. [Google Scholar]
  39. Aljourani, J.; Raeissi, K.; Golozar, M.A. Benzimidazole and its derivatives as corrosion inhibitors for mild steel in 1M HCl solution. Corros. Sci. 2009, 51, 1836–1843. [Google Scholar] [CrossRef]
  40. Ashassi Sorkhabi, H.; Shaabani, B.; Seifzadeh, D. Corrosion inhibition of mild steel by some Schiff base compounds in hydrochloric acid. Appl. Surf. Sci. 2005, 239, 154. [Google Scholar] [CrossRef]
  41. Moretti, G.; Guidi, F.; Grion, G. Tryptamine as a green iron corrosion inhibitor in 0.5 M deaerated sulphuric acid. Corros. Sci. 2004, 46, 387. [Google Scholar] [CrossRef]
  42. Cachet, C.; Keddam, M.; Mariotte, V.; Wiart, R. Influence of perfluorinated and hydrogenated surfactants upon hydrogen evolution on gold electrodes. Electrochim. Acta 1994, 39, 2743–2750. [Google Scholar] [CrossRef]
  43. Bentiss, F.; Bouanis, M.; Mernari, B.; Traisnel, M.; Vezin, H.; Lagrenee, M. Understanding the adsorption of 4H–1,2,4–triazole derivatives on mild steel surface in molar hydrochloric acid. Appl. Surf. Sci. 2006, 253, 3696–3703. [Google Scholar] [CrossRef]
  44. Negm, N.A.; Al Sabagh, A.M.; Migahed, M.A.; Abdel Bary, H.M.; El Din, H.M. Effectiveness of some diquaternary ammonium surfactants as corrosion inhibitors for carbon steel in 0.5 M HCl solution. Corros. Sci. 2010, 52, 2122–2132. [Google Scholar] [CrossRef]
  45. Behpour, M.; Ghoreishi, S.M.; Salavati-Niasari, M.; Ebrahimi, B. Evaluating two new synthesized S–N Schiff bases on the corrosion of copper in 15% hydrochloric acid. Mater. Chem. Phys. 2008, 107, 153–157. [Google Scholar] [CrossRef]
  46. Negm, N.A.; Ghuiba, E.M.; Mahmoud, S.A.; Tawfik, S.M. Biocidal and anti-corrosive activities of benzoimidazol-3-ium cationic Schiff base surfactants. Eng. Life Sci. 2011, 11, 496–510. [Google Scholar] [CrossRef]
  47. Tonthat, N.K.; Juvvadi, P.R.; Zhang, H.; Lee, S.C.; Venters, R.; Spicer, L.; Steinbach, W.J.; Heitman, J.; Schumacher, M.A. Structures of pathogenic fungal FKBP12s reveal possible self-catalysis function. MBio 2016, 7, e00492-16. [Google Scholar] [CrossRef] [Green Version]
  48. Borisova, A.S.; Eneyskaya, E.V.; Bobrov, K.S.; Jana, S.; Logachev, A.; Polev, D.E.; Lapidus, A.L.; Ibatullin, F.M.; Saleem, U.; Sandgren, M.; et al. Sequencing, biochemical characterization, crystal structure and molecular dynamics of cellobiohydrolase Cel7A from Geotrichum candidum 3C. FEBS J. 2015, 282, 4515–4537. [Google Scholar] [CrossRef]
  49. Rodríguez-Cárdenas, Á.; Rojas, A.L.; Conde-Giménez, M.; Velázquez-Campoy, A.; Hurtado-Guerrero, R.; Sancho, J. Streptococcus pneumoniae TIGR4 flavodoxin: Structural and biophysical characterization of a novel drug target. PLoS ONE 2016, 11, e0161020. [Google Scholar] [CrossRef] [Green Version]
  50. Li, H.J.; Li, X.; Liu, N.; Zhang, H.; Truglio, J.J.; Mishra, S.; Kisker, C.; Garcia-Diaz, M.; Tonge, P.J. Mechanism of the intramolecular Claisen condensation reaction catalyzed by MenB, a crotonase superfamily member. Biochemistry 2011, 50, 9532–9544. [Google Scholar] [CrossRef] [Green Version]
Figure 1. CA inhibition mechanism by sulfonamides.
Figure 1. CA inhibition mechanism by sulfonamides.
Materials 15 01146 g001
Figure 2. Metalo (II) 4-amino-benzenesulfonamide hydrogen complex.
Figure 2. Metalo (II) 4-amino-benzenesulfonamide hydrogen complex.
Materials 15 01146 g002
Figure 3. Variation in surface tension of surfactants IIa-c vs. concentration at 25 °C concentration expressed as mol/L.
Figure 3. Variation in surface tension of surfactants IIa-c vs. concentration at 25 °C concentration expressed as mol/L.
Materials 15 01146 g003
Figure 4. Polarization curves of carbon steel corrosion in 1 N HCl solution containing different concentrations of IIb inhibitor at 25 °C.
Figure 4. Polarization curves of carbon steel corrosion in 1 N HCl solution containing different concentrations of IIb inhibitor at 25 °C.
Materials 15 01146 g004
Figure 5. Image of the surface appearance of immersed samples in 1 M HCl by Scanning Electron Microscope (a) without inhibitor; and (bd) in the presence of 1 × 10−1 10, 1 × 10−2, 1 × 10−3 M IIb inhibitor, respectively.
Figure 5. Image of the surface appearance of immersed samples in 1 M HCl by Scanning Electron Microscope (a) without inhibitor; and (bd) in the presence of 1 × 10−1 10, 1 × 10−2, 1 × 10−3 M IIb inhibitor, respectively.
Materials 15 01146 g005
Figure 6. Docking energy scores (kcal/mol) for investigated compounds. ΔG: Free binding energy of the ligand from a given conformer; Int.: Affinity binding energy of hydrogen bond interaction with receptor; H.B.: Hydrogen bonding energy between protein and ligand; Eele: Electrostatic interaction with the receptor; Evdw: Van der Waals energies.
Figure 6. Docking energy scores (kcal/mol) for investigated compounds. ΔG: Free binding energy of the ligand from a given conformer; Int.: Affinity binding energy of hydrogen bond interaction with receptor; H.B.: Hydrogen bonding energy between protein and ligand; Eele: Electrostatic interaction with the receptor; Evdw: Van der Waals energies.
Materials 15 01146 g006
Figure 7. The Docked most active complexes into the electrostatic surface active sites of IDs: 4ZZt, 3T88, 5HWC and 5LJI using MOE tool [32].
Figure 7. The Docked most active complexes into the electrostatic surface active sites of IDs: 4ZZt, 3T88, 5HWC and 5LJI using MOE tool [32].
Materials 15 01146 g007
Table 1. The critical micelle concentration (CMC) and surface parameters of synthesized surfactants.
Table 1. The critical micelle concentration (CMC) and surface parameters of synthesized surfactants.
Comp. No.CMC X 10−3Γcmc (mN/m)Πcmc (mN/m)PC20 (Mole/L)Γmax X 10−11 (Mole/cm2)Amin (nm2)Δ GadsΔ GmicΔGads/Amin
IIa1.232403.910.41.5−67.7−34.1−46.8
IIb1.130424.110.21.5−69.9−34.8−49.1
IIc0.8029434.311.11.45−71.1−35.3−50.2
Table 2. Inhibition zone diameter (mm/mg sample) for the synthesized cationic surfactants against sulfate-reducing bacteria.
Table 2. Inhibition zone diameter (mm/mg sample) for the synthesized cationic surfactants against sulfate-reducing bacteria.
SampleInhibition Zone Diameter (Iz D)
(mm/mg Sample) Sulfate-Reducing Bacteria
IIa22
IIb20
IIc18
Table 3. Effect of cationic surfactant inhibitor concentration (IIb) at 30 °C temperature degrees.
Table 3. Effect of cationic surfactant inhibitor concentration (IIb) at 30 °C temperature degrees.
Temperature
°C
Conc. of Inhibitor
M
K
mg cm−2 h−2
ηw
%
300.001.307-
1 × 10−40.83835.86
5 × 10−40.64350.80
1 × 10−30.40269.26
5 × 10−30.29877.16
1 × 10−20.24181.54
Table 4. Effect of cationic surfactant inhibitor concentration (IIc) at 30 °C temperature degrees.
Table 4. Effect of cationic surfactant inhibitor concentration (IIc) at 30 °C temperature degrees.
Temperature
°C
Conc. of Inhibitor
M
K
mg cm−2 h−2
ηw
%
300.001.4-
1 × 10−40.561.82
5 × 10−40.26180.01
1 × 10−30.22283.01
5 × 10−30.10392.11
1 × 10−20.07094.68
Table 5. Electrochemical polarization parameters of carbon steel corrosion in the presence different concentrations of IIb and IIc inhibitors.
Table 5. Electrochemical polarization parameters of carbon steel corrosion in the presence different concentrations of IIb and IIc inhibitors.
Inhibitor NameConc. of Inhibitor (M)Ecorr (mV)Icorr (mAcm−2)βa (mV/Decade)βc (mV/Decade) θηP%
Without inhibitor0.00−487.32.02208.1202.4--
IIb1 × 10−4−499.00.0646118.0−137.40.7271.55
5 × 10−4−485.50.0345114.8−161.60.8584.81
1 × 10−3−485.40.0299137.2−194.20.8786.83
5 × 10−3−477.20.0280117.6−104.20.8887.67
1 × 10−2−504.70.0243128.1−140.30.8989.30
IIc1 × 10−4−563.60.0530116.5−176.30.7776.66
5 × 10−4−475.70.0315128.2−112.70.8686.13
1 × 10−3−478.80.0277127.6−106.30.8887.80
5 × 10−3−509.60.0244108.8−170.10.8989.26
1 × 10−2−496.90.0233125.8−196.50.9089.74
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Khowdiary, M.M.; Taha, N.A.; Saleh, N.M.; Elhenawy, A.A. Synthesis of Novel Nano-Sulfonamide Metal-Based Corrosion Inhibitor Surfactants. Materials 2022, 15, 1146. https://doi.org/10.3390/ma15031146

AMA Style

Khowdiary MM, Taha NA, Saleh NM, Elhenawy AA. Synthesis of Novel Nano-Sulfonamide Metal-Based Corrosion Inhibitor Surfactants. Materials. 2022; 15(3):1146. https://doi.org/10.3390/ma15031146

Chicago/Turabian Style

Khowdiary, Manal M., Nahla A. Taha, Nashwa M. Saleh, and Ahmed A. Elhenawy. 2022. "Synthesis of Novel Nano-Sulfonamide Metal-Based Corrosion Inhibitor Surfactants" Materials 15, no. 3: 1146. https://doi.org/10.3390/ma15031146

APA Style

Khowdiary, M. M., Taha, N. A., Saleh, N. M., & Elhenawy, A. A. (2022). Synthesis of Novel Nano-Sulfonamide Metal-Based Corrosion Inhibitor Surfactants. Materials, 15(3), 1146. https://doi.org/10.3390/ma15031146

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop