Next Article in Journal
Additive Manufacturing of AlSi10Mg and Ti6Al4V Lightweight Alloys via Laser Powder Bed Fusion: A Review of Heat Treatments Effects
Next Article in Special Issue
Study on the Surface of Cobalt-Chromium Dental Alloys and Their Behavior in Oral Cavity as Cast Materials
Previous Article in Journal
Development of 2.45 GHz Semiconductor Microwave System for Combustion Ignition Enhancement and Failure Analysis
Previous Article in Special Issue
Physicochemical Properties of Dentine Subjected to Microabrasive Blasting and Its Influence on Bonding to Self-Adhesive Prosthetic Cement in Shear Bond Strength Test: An In Vitro Study
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Increasing Acid Concentration, Time and Using a Two-Part Silane Potentiates Bond Strength of Lithium Disilicate–Reinforced Glass Ceramic to Resin Composite: An Exploratory Laboratory Study

1
Department of Conservative Dentistry, Instituto Universitário Egas Moniz (IUEM), Monte de Caparica, 2829-511 Almada, Portugal
2
Centro de Investigação Interdisciplinar Egas Moniz (CiiEM), Instituto Universitário Egas Moniz (IUEM), Monte de Caparica, 2829-511 Almada, Portugal
3
Division of Biomaterials and Tissue Engineering, Eastman Dental Institute, University College London (UCL), London NW3 2PF, UK
4
University Medical Center Groningen, Department of Restorative Dentistry and Biomaterials, Center for Dentistry and Oral Hygiene, University of Groningen, 9713 AV Groningen, The Netherlands
5
Department of Special Dental Care, Martini Hospital, 9728 NT Groningen, The Netherlands
6
Faculty of Health Sciences, University Arthuro Prat, Iquique 2120, Chile
*
Author to whom correspondence should be addressed.
Materials 2022, 15(6), 2045; https://doi.org/10.3390/ma15062045
Submission received: 11 January 2022 / Revised: 21 February 2022 / Accepted: 4 March 2022 / Published: 10 March 2022
(This article belongs to the Special Issue Surface Modification of Dental Materials and Tissues)

Abstract

:
There is still a lack of consensus concerning the recommended etching concentration, application time and type of silane when bonding lithium disilicate-reinforced glass ceramics manufactured by CAD/CAM. The purpose of this study was thus to conduct an in vitro study which investigates the influence of hydrofluoric acid (HF) concentration, etching time and silane type on the microtensile bond strength (μTBS) of lithium disilicate to resin composites. Thirty-nine IPS e.max CAD blocks were randomly divided between thirteen groups (n = 3). The variables were HF concentration (9.5 or 4.9%), etching time (20 or 60 s) and silane type (Bis-Silane, Monobond Plus and ESPE Sil Silane). The blocks were cut into beams, aged for 10,000 cycles in a thermocycler and submitted to tensile stress to determine μTBS. A control group featuring the Monobond Etch & Prime (MEP) agent that combines etching/silanisation into a simultaneous process was also added. This group was discarded from the analysis due to only having pre-test failures. The data were analysed using a three-way ANOVA (α = 0.05). The HF concentration, etching time and silane type significantly influenced μTBS (p < 0.001). Significant interactions between time and silane type (p = 0.004), HF concentration and silane type (p < 0.001) and among the three factors (p < 0.001) were noted. Etching lithium disilicate with 9.5% HF (60 s), followed by the application of Bis-Silane, resulted in the highest μTBS (16.6 ± 9.0 MPa). The highest concentration and etching time under study, combined with a two-part silane, resulted in the highest bond strength, while the application of MEP showed a complete pre-test failure.

1. Introduction

Lithium disilicate-reinforced glass ceramics are considered a strong and durable, yet esthetically minimally invasive, restorative option, since their glass matrix (in high vol%) allows them to be chemically treated and bonded to tooth substrates [1,2]. Their desirable biomechanical properties, such as high flexural strength and good fracture resistance, make them a popular choice in modern restorative dentistry [3]. This type of ceramic exhibits excellent biocompatibility and optical properties which are competitive with other ceramics, showing a 30% higher translucency than that of conventional zirconia [4,5]. Lithium disilicate ceramics can be made either by heat-pressing or in CAD/CAM milling devices and programs [6]. Lithium disilicate is considered one of the most versatile ceramic materials due to its high esthetics and good mechanical properties [7]. As such, it is widely-used in partial restorations, such as anterior veneers, posterior inlays, onlays and overlays, or in full coverage crowns and other complex fixed prostheses [4]. As such, with the aim of improving patient satisfaction by reducing the number of steps required to fabricate indirect restorations, thus saving chair time, these CAD/CAM systems are being used more often. This marks the adoption of a digital workflow philosophy which matches the technological advancements of the contemporary era [8,9].
It is essential for both the tooth and the ceramic to be surface-conditioned so that a satisfactory bond strength can be achieved, thereby increasing success rates. To do so, when lithium disilicate is considered, hydrofluoric acid etching and silane treatment are indispensable to achieve a micro-retentive surface, with high surface energy and stable chemical bonds. Such surface treatments have been established in the literature as mandatory to prepare ceramics with a high vol% of glass content [10,11,12]. However, a consensus on these protocols has not yet been reached, since etching times, concentrations and application time, or even type of silane, are highly variable among existing studies [13,14]. Clarification of these questions is therefore required.
When hydrofluoric acid (HF) is considered, it is important to understand that it is used to etch ceramics that have silica in their composition (i.e., a glass matrix), making HF useless for polycrystalline solids, such as zirconia. By creating micro-porosities that will serve as micro-retention sites, and also by increasing the energy surface tension, enhancing “wettability”, it substantially improves bond strength in a concentration and time-dependent manner [15,16]. Alternatively, silanes are subsequently used as coupling agents to achieve chemical bonds. These are bifunctional molecules containing a silicon atom (Si) bonded to three of the molecules’ alkoxy groups on one end (-Si-O-CH3), forming a hydrolysable ester group [17]. They contain an organofunctional methacrylate group able to react and co-polymerise with other methacrylate monomers, such as the ones present in the agent used for luting/bonding (adhesive, resin composite or luting cement). The alkoxy groups of the molecule rely on activation through hydrolysis. Therefore, they can condense, forming bonds with the silica-containing ceramic [17,18].
Complications arise when dealing with clinical choices, such as choosing the correct concentration of HF to use, which can range from 4.5 to 10% [19], or choosing the type of silane, which can come in one-part or a single bottle (pre-hydrolysed), or a two-part, non-hydrolysed system (containing a separate acid solution). Some authors found that simplified strategies resulted in poor adhesion, while others seem to favour their use [20,21]. Furthermore, deciding on the correct application time for etching or silanisation is also an extremely variable factor [13]. In fact, França et al. (2020) pointed out that there are substantial differences in chemical composition and microstructure across different lithium disilicate brands, which highlights the different etching times’ protocols [22]. Moreover, recently, some silane formulations and universal adhesive strategies also feature the functional monomer 10-methacryloyloxydecyl dihydrogen phosphate (10-MDP). As argued by some authors, 10-MDP could be favourable for increasing bond strengths in ceramic preparation protocols and could even be used as a silane hydrolyser component, due to its acidic nature, but a clear role is yet to be proven [23,24].
Thus, to elucidate on the best possible choice when surface treatments are required for bonding lithium disilicate, this study aims to evaluate the influence of HF concentration, surface etching time and type of silane used on the microtensile bond strength (μTBS) of a CAD/CAM lithium disilicate ceramic to resin composite. The null hypotheses were that (1) increasing the HF concentration (4.9 to 9.5%), (2) increasing the etching time or (3) varying the silane type do not influence the μTBS of CAD/CAM lithium disilicate-composites.

2. Materials and Methods

2.1. Materials

The materials used in this study, and their batch numbers and chemical compositions, are shown in Table 1. The samples under study were blocks of lithium disilicate-reinforced glass ceramics manufactured by CAD/CAM blocks (IPS e.max CAD, Ivoclar-Vivadent, Schaan, Liechtenstein). Thirty-nine IPS e.max blocks CAD A3-HT/C14 (12 mm × 14 mm × 7 mm) received a sintering heat treatment according to the instructions from the manufacturer (840–850 °C, Programat CS2, Ivoclar-Vivadent).

2.2. Sample Allocation and Preparation

The blocks were randomly distributed between thirteen groups (three blocks per group), according to a random number generation function (MS Excel, Microsoft, Redmond, WA, USA). Twelve groups were formed according to the experimental conditions under study: HF concentration (4.9 or 9.5%), etching time with HF (20 s or 60 s) and the type of silane coupling agent applied on the ceramic surface (Bis-Silane, Monobond Plus and ESPE Sil Silane Coupling Agent). The experimental design is shown in Figure 1.
Initially, the thirteenth group was tested using another commercial silane coupling agent—Monobond Etch & Prime (Table 1). This group was not etched with HF, nor was heat treatment of the silanised surface carried out (according to the instructions supplied by the manufacturer), since it combines both etching and silanisation into one process. This was followed by a thin adhesive layer of Optibond FL (Kerr, CA, USA), applied with a microbrush, gently air-dried for 3 s and not polymerised, in a manner equal to the other experimental groups. It was intended for comparison as a control group.
In all twelve groups, after HF etching, the samples were rinsed extensively for 20 s, and gently air-dried with an air-water syringe for 5 s. Post-etching cleaning was carried out using 35% orthophosphoric acid by actively rubbing the surface with a microbrush for 1 min (to clean the samples of extensive glass-matrix debris), then copiously rinsed with water for 20 s, gently air-dried with the air-water syringe for 5 s and finally placed in an ultrasonic bath for 5 min using distilled water. Silanisation was carried out according to the manufacturer′s instructions. For Bis-Silane, a single drop from each bottle was mixed at a 1:1 ratio, then one thin coat was applied and left to act for an additional 30 s. In the Monobond Plus group, a thin coat of silane was actively applied and allowed to act for 60 s. For the last silane system, ESPE Sil Silane Coupling Agent, a layer of silane was applied and subsequently left to dry for 5 min. After this, all of the samples (except for Monobond Etch & Prime) were heat-treated in a pre-heated oven at 100 °C for 1 min. Even though this is not specifically featured in the manufacturer instructions, the heating step was used in different studies and could enhance bond strengths [13,18]. For the consistency and reproducibility of the heat drying, an oven was used. A thin layer of the Optibond FL (Kerr, CA, USA) adhesive was applied with a microbrush for 15 s, gently air-dried for 3 s and was not polymerised.
To simulate a heated resin composite acting as a luting agent, an Enamel Plus HRi UD (Micerium S.p.A., Avegno, Ge, Italy) composite was pre-heated in an oven at 55 °C (ENA Heat Micerium S.p.A., Avegno, Ge, Italy) and packed on all specimens in increments of less than 2 mm of height, in a silicone mold. Each layer of resin was polymerised for 40 s with a high-intensity (1500 mW/cm2) LED unit (Elipar DeepCure-S, 3M ESPE AG, Seefeld, Germany) at a minimal distance. A pre-heated composite was chosen to bond samples as it is a restorative option used in modern adhesive dentistry, due to it having several advantages. These include vast shade choice, reduced solubility and shrinkage compared to conventional luting agents, good mechanical properties and a high degree of conversion [25,26]. The mean output intensity (>800 cm2) was verified regularly after every 3 exposures, using a radiometer—a Model 100 Curing Radiometer (Demetron Research Corporation, Dunbury, CT, USA).

2.3. Microtensile Bond Strength (μTBS) Test

The μTBS test was conducted in strict accordance with the guidelines published by the Academy of Dental Materials (2017) [27]. The samples were sectioned in a hard tissue microtome Accutom-50 (Struers A/S, Ballerup, Denmark) at low speed and under constant water cooling, to obtain beams with a cross-section of about 1 ± 0.2 mm2, which were then immersed in distilled water at 37 °C for 24 h before testing. A range of 50–80 beams per block were obtained. After water storage, the beams were subjected to 10,000 cycles between two water baths of 5 and 55 °C with a dwell time of 30 s in a THE-1100 thermocycler (SD Mechatronik GMBH, Feldkirchen-Westerham, Germany). The group featuring Monobond Etch & Prime had complete pre-test failures in all blocks, and as a result, was discarded before testing.
The beams were fixed to Geraldeli-type jigs with cyanoacrylate glue (Zapit, Dental Ventures of America, Corona, CA, USA). Each beam was tested at 0.5 mm/min until a failure in tension, in a universal testing machine using a 5 kN-load cell (Shimadzu Autograph AG-IS, Tokyo, Japan). For data analysis, all cohesive failures were discarded as they do not reflect the true value of bond strength at the interface, while pre-test failures (PTF) were included, considered as those with a microtensile bond strength value of 0 MPa [27].

2.4. Statistical Analysis

Data analysis was performed using IBM SPSS Statistics version 24.0 for Windows (IBM Corporation, Armonk, NY, USA), using descriptive and inferential statistics methods. Inferential analysis was carried out by using a factorial, three-way ANOVA model, considering the following fixed factors: HF concentration, etching time and silane type. Post-hoc multiple comparison analysis was performed using Tukey’s HSD test. Before the comparative analysis, the specimens’ microtensile bond strength values that were classified as outliers were removed and the factorial ANOVA model assumptions were validated. Estimated effect sizes, within the factorial model, were achieved by calculating the partial eta-squared coefficient (ƞ2p). The level of statistical significance was set at 5% for all inferential analyses.

3. Results

The means and standard errors of the microtensile bond strength values for each of the twelve experimental groups are presented in Table 2. The Monobond Etch & Prime group had complete pre-test failures in all blocks in the aging stage, and as a result, was discarded for posterior statistical analysis and comparison.
Inferential statistics were carried out by employing a three-way ANOVA model (Table 3), which confirmed that the microtensile bond strength was significantly influenced by the HF acid concentration (p < 0.001), surface acid etching time (p < 0.001) and type of silane applied (p < 0.001), with estimated effect sizes (ƞ2p) of 0.204, 0.064 and 0.031, respectively. Additionally, significant interactions were identified among the three factors (p < 0.001, ƞ2p = 0.058), between silane type and etching time (p = 0.004, ƞ2p = 0.013) and between HF acid concentration and silane type (p < 0.001, ƞ2p = 0.045). The interaction between HF acid concentration and etching time was not found to be significant (p = 0.074). In order to evaluate the differences in the average microtensile bond strengths among the groups, a multiple comparison analysis was conducted. The corresponding results are expressed in Table 2, along with the descriptive statistics results for the experimental groups.
The highest average μTBS values were obtained for the group where the surface of the lithium disilicate ceramic was etched with 9.5% HF acid for 60 s, followed by application of Bis-Silane (16.6 ± 9.0 MPa). The lowest average μTBS values were obtained for the system using the ESPE Sil Silane Coupling Agent, with a 4.9% HF acid concentration and a 20 s etching time (0.6 ± 1.0 MPa).
The results of failure analysis are presented in Table 4. All specimens obtained for the Monobond Etch & Prime group had pre-test failure. For the experimental groups, the predominant fracture mode was mixed for the groups in which the ceramic surface was etched with 9.5% HF acid, ranging from 51.9 to 82.1% of total fractures. In groups where the ceramic surface was etched with 4.9% HF acid, the failure mode distribution varied strongly, depending on the silane system that was applied.

4. Discussion

The study confirmed the significant impact of choosing the correct concentration, etching time and type of silane, as the three variables in this study had a significant influence on the μTBS values of the ceramic–resin interface. Ageing the specimens artificially is particularly important in this study design as it is possible to mimic in laboratory settings, with the thermally-induced mechanical fatigue phenomena (due to thermal expansion) and the hydrolytic degradation in the indirect restorative bonded interface designed to last a long time [28].
Lithium disilicate-reinforced glass ceramics, according to the instructions supplied by the manufacturer, should be etched with 4.9% HF over a period of 20 s to minimise damage to the ceramic surface. However, a better surface conditioning pattern for lithium disilicate has been previously observed, with HF etching at 9.5% for 60 s, showing that it benefits from increases in time and concentration, as also confirmed in this study [29]. A study from Soares et al. (2005) also reported that HF at 9.5% for 20 s is effective in removing the second crystalline phase and glassy matrix from lithium disilicate-reinforced glass ceramics, resulting in an appropriate bonding surface which is subsequently receptive to resin composites [30]. In the present study, the microtensile bond strength results were found to be significantly higher when the ceramic surface was etched for 60 s (at a 9.5% concentration) using Bis-Silane. These results suggest that a longer etching time leads to an increased surface roughness, facilitating micromechanical retention and, consequently, higher bond strengths with adherends, agreeing with several other studies [12,31]. This concentration may not affect the flexural strength of the network [32]. In addition, as seen from the results of this study, the concentration of the etchant was the factor which had the biggest effect size, in comparison to the etching time and type of silane, implying that a greater dissolution of the glassy matrix, owing to greater etching aggressiveness, is linked to higher bond strengths. This, of course, is linked to the appropriate silane choice. These results should only be taken into account when the composition and thickness of the ceramic under use is also considered [19,22]. Chemical surface modification occurs after HF etching, with LiSiF nano-precipitates forming on the L i 2 S i 2 O 5 needles, having changed from a crystal morphology. These needles can then improve bonding with the silane and provide additional nano-roughness on the free surface, with a consequent densification of the three-dimensional siloxane network [33].
The choice of silane was also crucial as it directly affected the bond strength of the resulting interface. The results obtained in this study agree with those reported by Kalavacharla et al. (2015), with the highest μTBS results obtained with Bis-Silane [12]. These results can be explained by the fact that Bis-Silane is a two-part non-hydrolysed silane solution. The activation of the silane occurs upon mixing the content of the two bottles. In contrast, with pre-hydrolysed silanes, hydrolysis has already taken place since the acidic component is mixed with the silane in the same bottle, and some pre-condensation phenomena may have already occurred when the clinician applies the system. Thus, such solutions, when they are bought and used by the clinician, may contain residual silane monomers which have reacted and associated, forming oligomers that are no longer able to establish chemical bonds [17,18]. Nevertheless, pre-hydrolysed silanes are considered stable solutions even though their shelf life is considered inferior to two-component silane systems. Turning to two-component silane systems, their hydrolysis mechanisms, upon mixing, do not reach their peak in a clinically relevant application time [34].
Regarding Monobond Plus, the 10-MDP present in its composition increases the potential for chemical interactions with different surfaces. In the present study, the results obtained from the experimental groups in which Monobond Plus was applied could suggest that the addition of 10-MDP was not significant enough to compete with other silane strategies. Non-conclusive results can also be found in the literature, since some say 10-MDP may enhance the hydrolytic stability of silanes [23]. Furthermore, the acidic media created by 10-MDP is stronger in hydrolyzing silane molecules than acetic acid, forming strong siloxane bonds (-Si-O-Si) on the surface of the silica-based ceramic [35,36]. Such interactions may also result in a limitation of the self-dehydration condensation for silane molecules, through MDP hydrolysis, increasing the number of silane-ceramic bonds [24].
The lowest microtensile bond strength result was obtained in the group where ESPE Sil was applied, with an HF application at 4.9% for 20 s. This result was possibly a consequence of the pre-hydrolysis of the silane combined with the insufficient etching of the glass-ceramic. ESPE Sil is intentionally used to function as a coupling agent to silica-coated materials. In etched lithium disilicate, fewer silica-containing surfaces could be presented, and therefore its use as a silane in such circumstances could be less effective. As stated above, one major disadvantage of this type of silane is the rapid formation of oligomers without coupling ability, thus impairing the strength of the adhesive interface. The high number of pre-test failures (52.1%) in this group and its quantification at 0 MPa also contributed to the lower values for bond strength. Low values due to insufficient surface treatments provided to comparable substrates have been reported [37]. Conversely, with other silanes, failures were well distributed among the different classifications.
Monobond Etch & Prime was introduced as a single-bottle alternative to the HF etching and silane application in separate steps. It is considered a self-etching silane. It contains tetrabutyl ammonium dihydrogen trifluoride (TADF), a methacrylate phosphate monomer and a methacrylate-functionalised silane [38]. TADF is an acid salt generally used for etching silica in the surface of glass ceramics, to obtain a rough surface for micromechanical retention. TADF is a much weaker acid compared to HF, so a weaker etching pattern is expected. In fact, previous studies have proved that the resulting roughness of lithium disilicate surfaces after use of this silane, in comparison to HF etching, is substantially lower. Additionally, the authors in the same study reported that the bond strength of Monobond Etch & Prime was even lower than the negative control group after ageing [38]. Other authors also corroborated a lower roughening and etching efficacy on the surface of lithium disilicate-reinforced glass ceramics when this silane was applied, compared to traditional HF and lower shear bond strengths [39]. These results are also similar to Lopes et al. (2018) and Swank et al. (2018), which found the simplified strategy presented the lowest bond strengths and predominantly adhesive failures [20,40]. Other studies, however, observed a good adhesive performance with this ceramic conditioning agent [41,42,43]. It should be noted that, in one of the studies, the surface of the ceramic was roughened beforehand, which may have contributed to the better bond strength results, and a macrotensile setup was used as opposed to microtensile [40]. In the present study, the group in which Monobond Etch & Prime was applied may have prematurely failed due to the lack of micromechanical retention, and thus, the resulting bond strength was not enough for the samples to withstand being sectioned into beams. Micromechanical retention and surface roughness are paramount to achieve acceptable bond strengths with CAD/CAM materials [44]. Adhesion may have also been compromised, because the protocol of this new product requires the silane to be rinsed after it is applied. Moreover, following the instructions from the manufacturer, the silane heat treatment was not performed. This treatment allows for the elimination of contaminants, such as water and alcohol, that affect adhesion [18]. The heat additionally promotes the condensation reaction between silica and silane, and promotes the formation of more resistant bonds between the ceramic surface and the silane. As mentioned, it is important to stress that the use of silane shows contradictory results in the literature.
It is important to point out that silanisation is considered to be a technique-sensitive procedure. The instructions provided by manufacturers all display highly different application times and modes. Moreover, the temperature used when carrying out heat treatment demonstrates extreme variabilities in time, range and heat mode, which can range from as low as 5 s up to 2 min, performed at room temperature or heated to 100 °C. Heat treatments can also be performed in several different ways (from using air dryers to a toaster oven). As stated by Bruzi et al. (2017), an urgent need for standardisation arises, so as to inform clinicians on what the best practical approach may be in regard to silane treatment [13]. Optimal silane application is a crucial factor in guaranteeing not only immediate bond strength results, but also their stability [28]. In addition, pre-hydrolysed solutions with acidic components, such as acetic acid or phosphate group-containing monomers, may acidify over time, contributing to the instability of the system [45,46]. All of these remarks could also potentially explain the differences between the tested silanes.
A few possible study limitations should be pointed out. This study lacked a non-thermocycled group comparison because the aim was to test aged interfaces only. This, however, would have provided additional information regarding the role of hydrolysis mechanisms in different types of silane treatments in ceramic–resin interfaces, and should be carried out in the future. Moreover, heat treatment could have been carried out in the Monobond Etch & Prime group to standardise all silane groups. It is uncertain whether this would have improved its results. Nonetheless, it was decided to follow the manufacturer instructions for all tested materials.

5. Conclusions

The longer etching times, performed in higher concentrations, associated with two-part silanes resulted in the best approach for aged μTBS data. Specifically, etching the surface of the lithium disilicate ceramic with 9.5% HF for 60 s, followed by the application of Bis-Silane, produced the highest μTBS. The lowest average μTBS values were obtained for the ESPE Sil Silane Coupling Agent system (4.9% HF, 20 s). According to the microtensile behaviour obtained in this laboratory study for Monobond Etch & Prime, with all specimens experiencing pre-test failure, and considering all the limitations in the study design, clinical use should be cautious until further evidence is available. This study raises additional doubts concerning simplified silanisation strategies.

Author Contributions

Conceptualisation, M.A., J.J.M., J.R. and M.M.M.G.; methodology, A.H.S.D., I.C.S., L.P., J.J.M. and M.M.M.G.; software, P.M. and L.P.; validation, A.H.S.D., J.R. and M.M.M.G.; formal analysis, A.H.S.D., I.C.S., L.P. and M.M.M.G.; investigation, M.A. and B.M.; resources, P.M.; data curation, M.A., B.M., A.H.S.D. and I.C.S.; writing—original draft preparation, M.A., B.M., A.H.S.D. and L.P.; writing—review and editing, A.H.S.D. and M.M.M.G.; supervision, J.R. and M.M.M.G.; project administration, P.M., J.R. and J.J.M. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Data may be available upon request from the author.

Acknowledgments

The authors acknowledge Egas Moniz Cooperativa de Ensino Superior, C.R.L. for their support in this research work.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Özcan, M.; Dündar, M.; Erhan Çömlekoğlu, M. Adhesion concepts in dentistry: Tooth and material aspects. J. Adhes. Sci. Technol. 2012, 26, 2661–2681. [Google Scholar] [CrossRef] [Green Version]
  2. Giordano, R.; McLaren, E. Ceramics overview: Classification by microstructure and processing methods. Compend. Contin. Educ. Dent. 2010, 31, 18–30. [Google Scholar]
  3. Ho, G.W.; Matinlinna, J.P. Insights on Ceramics as Dental Materials. Part I: Ceramic Material Types in Dentistry. Silicon 2011, 3, 109–115. [Google Scholar] [CrossRef] [Green Version]
  4. Zarone, F.; Di Mauro, M.I.; Ausiello, P.; Ruggiero, G.; Sorrentino, R. Current status on lithium disilicate and zirconia: A narrative review. BMC Oral Health 2019, 19, 1–14. [Google Scholar] [CrossRef] [Green Version]
  5. Baldissara, P.; Llukacej, A.; Ciocca, L.; Valandro, F.L.; Scotti, R. Translucency of zirconia copings made with different CAD/CAM systems. J. Prosthet. Dent. 2010, 104, 6–12. [Google Scholar] [CrossRef]
  6. Li, R.W.K.; Chow, T.W.; Matinlinna, J.P. Ceramic dental biomaterials and CAD/CAM technology: State of the art. J. Prosthodont. Res. 2014, 58, 208–216. [Google Scholar] [CrossRef] [Green Version]
  7. Fabian Fonzar, R.; Carrabba, M.; Sedda, M.; Ferrari, M.; Goracci, C.; Vichi, A. Flexural resistance of heat-pressed and CAD-CAM lithium disilicate with different translucencies. Dent. Mater. 2017, 33, 63–70. [Google Scholar] [CrossRef]
  8. Zandinejad, A.; Lin, W.S.; Atarodi, M.; Abdel-Azim, T.; Metz, M.J.; Morton, D. Digital Workflow for Virtually Designing and Milling Ceramic Lithium Disilicate Veneers: A Clinical Report. Oper. Dent. 2015, 40, 241–246. [Google Scholar] [CrossRef]
  9. Sailer, I.; Benic, G.I.; Fehmer, V.; Hämmerle, C.H.F.; Mühlemann, S. Randomized controlled within-subject evaluation of digital and conventional workflows for the fabrication of lithium disilicate single crowns. Part II: CAD-CAM versus conventional laboratory procedures. J. Prosthet. Dent. 2017, 118, 43–48. [Google Scholar] [CrossRef] [Green Version]
  10. Magne, P.; Razaghy, M.; Carvalho, M.A.; Soares, L.M. Luting of inlays, onlays, and overlays with preheated restorative composite resin does not prevent seating accuracy. Int. J. Esthet. Dent. 2018, 13, 318–332. [Google Scholar]
  11. Krummel, A.; Garling, A.; Sasse, M.; Kern, M. Influence of bonding surface and bonding methods on the fracture resistance and survival rate of full-coverage occlusal veneers made from lithium disilicate ceramic after cyclic loading. Dent. Mater. 2019, 35, 1351–1359. [Google Scholar] [CrossRef] [PubMed]
  12. Kalavacharla, V.K.; Lawson, N.C.; Ramp, L.C.; Burgess, J.O.; Kalavacharla, V.K.; Lawson, N.C.; Burgess, J.O. Influence of Etching Protocol and Silane Treatment with a Universal Adhesive on Lithium Disilicate Bond Strength. Oper. Dent. 2015, 40, 372–378. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  13. Bruzi, G.; Carvalho, A.O.; Giannini, M.; Maia, H.P.; Magne, P. Post-etching cleaning influences the resin shear bond strength to CAD/CAM lithium-disilicate ceramics. Appl. Adhes. Sci. 2017, 5, 17. [Google Scholar] [CrossRef] [Green Version]
  14. Rita, A.; Reis, J.; Santos, I.C.; Delgado, A.H.S.; Rua, J.; Proença, L.; Mendes, J.J. Influence of silane type and application time on the bond strength to leucite reinforced ceramics. Ann. Med. 2021, 53, S50–S51. [Google Scholar] [CrossRef]
  15. Puppin-Rontani, J.; Sundfeld, D.; Costa, A.R.; Correr, A.B.; Puppin-Rontani, R.M.; Borges, G.A.; Sinhoreti, M.A.C.; Correr-Sobrinho, L. Effect of Hydrofluoric Acid Concentration and Etching Time on Bond Strength to Lithium Disilicate Glass Ceramic. Oper. Dent. 2017, 42, 606–615. [Google Scholar] [CrossRef]
  16. Prochnow, C.; Venturini, A.B.; Grasel, R.; Gundel, A.; Bottino, M.C.; Valandro, L.F. Adhesion to a Lithium Disilicate Glass Ceramic Etched with Hydrofluoric Acid at Distinct Concentrations. Braz. Dent. J. 2018, 29, 492–499. [Google Scholar] [CrossRef]
  17. Lung, C.Y.K.; Matinlinna, J.P. Aspects of silane coupling agents and surface conditioning in dentistry: An overview. Dent. Mater. 2012, 28, 467–477. [Google Scholar] [CrossRef]
  18. Matinlinna, J.P.; Lung, C.Y.K.; Tsoi, J.K.H. Silane adhesion mechanism in dental applications and surface treatments: A review. Dent. Mater. 2018, 34, 13–28. [Google Scholar] [CrossRef]
  19. Garfias, C.S.; De Goes, M.F. Dissolution Depth and Surface Morphological Alterations in Ultrathin Glass Ceramic Etched with Different Hydrofluoric Acid -etching Protocols. J. Adhes. Dent. 2021, 23, 579–587. [Google Scholar] [CrossRef]
  20. Lopes, G.; Perdigão, J.; Baptista, D.; Ballarin, A. Does a Self-Etching Ceramic Primer Improve Bonding to Lithium Disilicate Ceramics? Bond Strengths and FESEM Analyses. Oper. Dent. 2018, 44, 210–218. [Google Scholar] [CrossRef]
  21. Dimitriadi, M.; Zafiropoulou, M.; Zinelis, S.; Silikas, N.; Eliades, G. Silane reactivity and resin bond strength to lithium disilicate ceramic surfaces. Dent. Mater. 2019, 35, 1082–1094. [Google Scholar] [CrossRef] [PubMed]
  22. França, R.; Bebsh, M.; Haimeur, A.; Fernandes, A.C.; Sacher, E. Physicochemical surface characterizations of four dental CAD/CAM lithium disilicate-based glass ceramics on HF etching: An XPS study. Ceram. Int. 2020, 46, 1411–1418. [Google Scholar] [CrossRef]
  23. Cardenas, A.M.; Siqueira, F.; Hass, V.; Malaquias, P.; Gutierrez, M.F.; Reis, A.; Perdigão, J.; Loguercio, A.D. Effect of MDP-containing Silane and Adhesive Used Alone or in Combination on the Long-term Bond Strength and Chemical Interaction with Lithium Disilicate Ceramics. J. Adhes. Dent. 2017, 19, 203–212. [Google Scholar] [CrossRef]
  24. Maruo, Y.; Nishigawa, G.; Yoshihara, K.; Minagi, S.; Matsumoto, T.; Irie, M. Does 8-methacryloxyoctyl trimethoxy silane (8-MOTS) improve initial bond strength on lithium disilicate glass ceramic? Dent. Mater. 2017, 33, e95–e100. [Google Scholar] [CrossRef] [PubMed]
  25. Bortolotto, T.; Guillarme, D.; Gutemberg, D.; Veuthey, J.L.; Krejci, I. Composite resin vs resin cement for luting of indirect restorations: Comparison of solubility and shrinkage behavior. Dent. Mater. J. 2013, 32, 834–838. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  26. Lopes, L.C.P.; Terada, R.S.S.; Tsuzuki, F.M.; Giannini, M.; Hirata, R. Heating and preheating of dental restorative materials—a systematic review. Clin. Oral Investig. 2020, 24, 4225–4235. [Google Scholar] [CrossRef] [PubMed]
  27. Armstrong, S.; Breschi, L.; Özcan, M.; Pfefferkorn, F.; Ferrari, M.; Van Meerbeek, B. Academy of Dental Materials guidance on in vitro testing of dental composite bonding effectiveness to dentin/enamel using micro-tensile bond strength (μTBS) approach. Dent. Mater. 2017, 33, 133–143. [Google Scholar] [CrossRef] [Green Version]
  28. Magne, P.; Bruzi, G.; Carvalho, A.; Enciso, R.; Giannini, M. Optimization of Heat-Dried Silane Application for CAD/CAM Ceramic Resin Bonding. Nanosci. Nanotechnol. 2018, 2. [Google Scholar] [CrossRef]
  29. Ramakrishnaiah, R.; Alkheraif, A.A.; Divakar, D.D.; Matinlinna, J.P.; Vallittu, P.K. The Effect of Hydrofluoric Acid Etching Duration on the Surface Micromorphology, Roughness, and Wettability of Dental Ceramics. Int. J. Mol. Sci. 2016, 17, 822. [Google Scholar] [CrossRef] [Green Version]
  30. Soares, C.J.; Soares, P.V.; Pereira, J.C.; Fonseca, R.B. Surface treatment protocols in the cementation process of ceramic and laboratory-processed composite restorations: A literature review. J. Esthet. Restor. Dent. 2005, 17, 224–235. [Google Scholar] [CrossRef]
  31. Chen, J.H.; Matsumura, H.; Atsuta, M. Effect of different etching periods on the bond strength of a composite resin to a machinable porcelain. J. Dent. 1998, 26, 53–58. [Google Scholar] [CrossRef]
  32. Menees, T.S.; Lawson, N.C.; Beck, P.R.; Burgess, J.O. Influence of particle abrasion or hydrofluoric acid etching on lithium disilicate flexural strength. J. Prosthet. Dent. 2014, 112, 1164–1170. [Google Scholar] [CrossRef] [PubMed]
  33. Poulon-Quintin, A.; Ogden, E.; Large, A.; Vaudescal, M.; Labrugère, C.; Bartala, M.; Bertrand, C. Chemical surface modification of lithium disilicate needles of a silica-based ceramic after HF-etching and ultrasonic bath cleaning: Impact on the chemical bonding with silane. Dent. Mater. 2021, 37, 832–839. [Google Scholar] [CrossRef]
  34. Delgado, A.H.; Reis, J.; Rita, A.; Caetano Santos, I.; Rua, J.; Proença, L.; Mendes, J.J. Silane coupling agent type and application time influences the bond strength of resin-feldspathic CAD/CAM ceramics. Restor. Dent. Endod. 2019, 44, OP-21. [Google Scholar]
  35. Yu, H.; Yoshida, K.; Cheng, H.; Sawase, T. Bonding of different self-adhesive resins to high-strength composite resin block treated with surface conditioning. J. Prosthodont. Res. 2019, 63, 340–346. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  36. Koko, M.; Takagaki, T.; Abdou, A.; Inokoshi, M.; Ikeda, M.; Wada, T.; Uo, M.; Nikaido, T.; Tagami, J. Effects of the ratio of silane to 10-methacryloyloxydecyl dihydrogenphosphate (MDP) in primer on bonding performance of silica-based and zirconia ceramics. J. Mech. Behav. Biomed. Mater. 2020, 112, 104026. [Google Scholar] [CrossRef]
  37. Bruzi, G.; Carvalho, A.O.; Giannini, M.; Maia, H.P.; Magne, P. Bonding of CAD/CAM lithium disilicate restorations with regular and flowable composite resin with and without wetting resin. Appl. Adhes. Sci. 2018, 6, 1–9. [Google Scholar] [CrossRef] [Green Version]
  38. Dimitriadi, M.; Zinelis, S.; Zafiropoulou, M.; Silikas, N.; Eliades, G. Self-Etch Silane Primer: Reactivity and Bonding with a Lithium Disilicate Ceramic. Materials 2020, 13, 641. [Google Scholar] [CrossRef] [Green Version]
  39. El-Damanhoury, H.M.; Gaintantzopoulou, M.D. Self-etching ceramic primer versus hydrofluoric acid etching: Etching efficacy and bonding performance. J. Prosthodont. Res. 2018, 62, 75–83. [Google Scholar] [CrossRef]
  40. Swank, H.M.; Motyka, N.C.; Bailey, C.W.; Vandewalle, K.S. Bond strength of resin cement to ceramic with simplified primers and pretreatment solutions-PubMed. Gen. Dent. 2018, 66, 33–37. [Google Scholar]
  41. Lyann, S.K.; Takagaki, T.; Nikaido, T.; Uo, M.; Ikeda, M.; Sadr, A.; Tagami, J. Effect of Different Surface Treatments on the Tensile Bond Strength to Lithium Disilicate Glass Ceramics. J. Adhes. Dent. 2018, 20, 261–268. [Google Scholar] [CrossRef] [PubMed]
  42. Wille, S.; Lehmann, F.; Kern, M. Durability of Resin Bonding to Lithium Disilicate and Zirconia Ceramic using a Self-etching Primer. J. Adhes. Dent. 2017, 19, 491–496. [Google Scholar] [CrossRef] [PubMed]
  43. Dapieve, K.S.; Aragonez, G.C.; Prochnow, C.; Burgo, T.A.d.L.; Rippe, M.P.; Pereira, G.K.R.; Venturini, A.B.; Valandro, L.F. Different Etching Times of a One-step Ceramic Primer: Effect on the Resin Bond Strength Durability to a CAD/CAM Lithium-Disilicate Glass-Ceramic. J. Adhes. Dent. 2021, 23, 133–143. [Google Scholar] [CrossRef] [PubMed]
  44. Güngör, M.B.; Nemli, S.K.; Bal, B.T.; Ünver, S.; Dogan, A. Effect of surface treatments on shear bond strength of resin composite bonded to CAD/CAM resin-ceramic hybrid materials. J. Adv. Prosthodont. 2016, 8, 259–266. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  45. Yao, C.; Yu, J.; Wang, Y.; Tang, C.; Huang, C. Acidic pH weakens the bonding effectiveness of silane contained in universal adhesives. Dent. Mater. 2018, 34, 809–818. [Google Scholar] [CrossRef]
  46. Zakir, M.; Tsoi, J.K.H.; Chu, C.H.; Lung, C.Y.K.; Matinlinna, J.P. Bonding Dissimilar Materials in Dentistry: A Critical Review. Rev. Adhes. Adhes. 2014, 2, 413–432. [Google Scholar] [CrossRef]
Figure 1. Experimental design featuring block preparation, random allocation and division according to the three variables under study.
Figure 1. Experimental design featuring block preparation, random allocation and division according to the three variables under study.
Materials 15 02045 g001
Table 1. Materials used in the study (information as disclosed by the manufacturers).
Table 1. Materials used in the study (information as disclosed by the manufacturers).
MaterialTypeManufacturerBatch No.Composition
IPS Ceramic
Etching Gel
EtchantIvoclar-Vivadent,
Schaan, Liechtenstein
T29351Hydrofluoric acid 4.9%
Porcelain Etchant 9.5%EtchantBisco Inc.,
Schaumburg, IL, USA
1600002039Aqueous solution of hydrofluoric acid (9.5%), 50–70% polyacrylamidomethylpropane sulfonic acid
sodium fluoride
Bis-SilaneSilaneBisco, Schaumburg,
IL, USA
1600001184
1600001185
Part A: >85% ethanol,
5–10% 3-(Trimethoxysilyl) propyl-2-methyl-2-propenoic acid
Part B: 30–50% ethanol,
1–5% phosphoric acid
Monobond PlusSilaneIvoclar-Vivadent,
Schaan, Liechtenstein
V2126650–100% ethanol, disulfit
methacrylate, ≤2.5% phosphoric
acid dimethacrylate, ≤2.5% 3-trimethoxysilylpropyl methacrylate
ESPE Sil
Silane Coupling
Agent
Silane3M ESPE AG,
Seefeld, Germany
632307>97% ethanol, <3% 3-trimethoxysilylpropyl methacrylate,
<2% methyl ethyl ketone
Monobond Etch
& Prime
SilaneIvoclar-Vivadent,
Schaan, Liechtenstein
W0561910–25% butanol, 2.5–10% tetrabutyl ammonium dihydrogen trifluoride, methacrylated phosphoric acid ester, <2.5% bis(triethoxysilyl) ethane
Optibond FLBonding agentKerr, CA, USA6158322Adhesive: Bis-GMA,
HEMA, GDMA, CQ,
ODMAB, fillers (~48%)
Resin
Composite
Enamel Plus HRi
CompositeMicerium S.p.A.,
Avegno, Ge, Italy
2017000418
2016001162
2016008171
UDMA, Bis-GMA,
Butanediol, Dimethacrylate,
Glass fillers, Zirconia oxide
nanoparticles
Lithium
disilicate
ceramic IPS
e.max CAD
A3-HT/C14
CeramicIvoclar-Vivadent,
Schaan, Liechtenstein
V49313SiO2, Li2O, K2O, MgO,
Al2O3, P2O5, other oxides
* Percentages of components are shown in weight%. Legend: Bis-GMA: Bisphenol-A glycidyl dimethacrylate; CQ: camphorquinone; GDMA: 1,3-glycerol dimethacrylate; ODMAB: 2-(ethylhexyl)-4-(dimethylamino)benzoate; UDMA: urethane dimethacrylate.
Table 2. μTBS values (MPa) after 10,000 thermocycles (artificial aging) for the tested groups, presented as mean (M) ± standard error (SE). Total number of specimens (n). Monobond Etch & Prime was excluded from this table since this group had a complete pre-test failure, and thus its bond strengths could not be measured.
Table 2. μTBS values (MPa) after 10,000 thermocycles (artificial aging) for the tested groups, presented as mean (M) ± standard error (SE). Total number of specimens (n). Monobond Etch & Prime was excluded from this table since this group had a complete pre-test failure, and thus its bond strengths could not be measured.
Bis-SilaneMonobond PlusESPE Sil Silane CA
HF Ac. Conc. (%)Etching Time (s)nM ± SEnM ± SEnM ± SE
9.520667.0 ± 0.5 aA6410.4 ± 0.8 aBC7912.4 ± 0.9 aB
607616.6 ± 1.0 bA6912.3 ± 0.7 aB7812.4 ± 0.8 aB
4.920748.5 ± 0.7 aA734.8 ± 0.4 bB530.6 ± 0.1 bC
60728.9 ± 0.7 aA716.8 ± 0.4 cAB805.5 ± 0.6 cB
* Different lower-case letters indicate significant differences between means in the same column, and different upper-case letters indicate significant differences between means in the same row (Tukey HSD post-hoc test, p < 0.05).
Table 3. Three-way ANOVA results, considering the factors: HF acid concentration, etching time and silane type.
Table 3. Three-way ANOVA results, considering the factors: HF acid concentration, etching time and silane type.
SourceType III Sum of SquaresdfMean SquareFp
Model13,683.276111243.93435.380<0.001
HF acid concentration7599.03917599.039216.129<0.001
Etching time2017.63512017.63557.385<0.001
Silane type956.5922478.29613.604<0.001
HF acid concentration × etching time 112.8291112.8293.2090.074
Etching time × silane type388.3752194.1985.5230.004
HF acid concentration × silane type 1405.8892702.94419.993<0.001
HF acid concentration × etching time × silane type1821.6572910.82825.905<0.001
Error29,604.43184235.160
Total113,456.851854
Table 4. Failure distribution (% within group), as a function of HF acid concentration, etching time and silane type (A—Adhesive, M—Mixed, C—Cohesive, PTF—Pre-test failure).
Table 4. Failure distribution (% within group), as a function of HF acid concentration, etching time and silane type (A—Adhesive, M—Mixed, C—Cohesive, PTF—Pre-test failure).
Bis-SilaneMonobond PlusESPE Sil Silane Coupling Agent
HF Ac. Conc. (%)Etching Time (s)AMCPTFAMCPTFAMCPTF
9.52025.045.017.512.528.455.26.010.413.675.32.58.6
6029.951.916.91.323.062.214.90.013.182.10.04.8
4.92051.329.51.317.922.254.30.023.546.61.40.052.1
6038.543.61.316.722.267.91.28.659.010.81.228.9
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Almiro, M.; Marinho, B.; Delgado, A.H.S.; Rua, J.; Monteiro, P.; Santos, I.C.; Proença, L.; Mendes, J.J.; Gresnigt, M.M.M. Increasing Acid Concentration, Time and Using a Two-Part Silane Potentiates Bond Strength of Lithium Disilicate–Reinforced Glass Ceramic to Resin Composite: An Exploratory Laboratory Study. Materials 2022, 15, 2045. https://doi.org/10.3390/ma15062045

AMA Style

Almiro M, Marinho B, Delgado AHS, Rua J, Monteiro P, Santos IC, Proença L, Mendes JJ, Gresnigt MMM. Increasing Acid Concentration, Time and Using a Two-Part Silane Potentiates Bond Strength of Lithium Disilicate–Reinforced Glass Ceramic to Resin Composite: An Exploratory Laboratory Study. Materials. 2022; 15(6):2045. https://doi.org/10.3390/ma15062045

Chicago/Turabian Style

Almiro, Matilde, Beatriz Marinho, António H. S. Delgado, João Rua, Paulo Monteiro, Inês Caetano Santos, Luís Proença, José João Mendes, and Marco M. M. Gresnigt. 2022. "Increasing Acid Concentration, Time and Using a Two-Part Silane Potentiates Bond Strength of Lithium Disilicate–Reinforced Glass Ceramic to Resin Composite: An Exploratory Laboratory Study" Materials 15, no. 6: 2045. https://doi.org/10.3390/ma15062045

APA Style

Almiro, M., Marinho, B., Delgado, A. H. S., Rua, J., Monteiro, P., Santos, I. C., Proença, L., Mendes, J. J., & Gresnigt, M. M. M. (2022). Increasing Acid Concentration, Time and Using a Two-Part Silane Potentiates Bond Strength of Lithium Disilicate–Reinforced Glass Ceramic to Resin Composite: An Exploratory Laboratory Study. Materials, 15(6), 2045. https://doi.org/10.3390/ma15062045

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop