Next Article in Journal
Fabricated Flexible Composite for a UV-LED Color Filter and Anti-Counterfeiting Application of Calcium Molybdate Phosphor Synthesized at Room Temperature
Next Article in Special Issue
Ignition and Combustion Characteristic of B·Mg Alloy Powders
Previous Article in Journal
An Inverse Analysis for Establishing the Temperature-Dependent Thermal Conductivity of a Melt-Cast Explosive across the Whole Solidification Process
Previous Article in Special Issue
Achieving High-Strength and Toughness in a Mg-Gd-Y Alloy Using Multidirectional Impact Forging
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Effect of the Ca2Mg6Zn3 Phase on the Corrosion Behavior of Biodegradable Mg-4.0Zn-0.2Mn-xCa Alloys in Hank’s Solution

Faculty of Materials and Manufacturing, Beijing University of Technology, Beijing 100124, China
*
Authors to whom correspondence should be addressed.
Materials 2022, 15(6), 2079; https://doi.org/10.3390/ma15062079
Submission received: 17 January 2022 / Revised: 25 February 2022 / Accepted: 7 March 2022 / Published: 11 March 2022

Abstract

:
The effect of the Ca2Mg6Zn3 phase on the corrosion behavior of biodegradable Mg-4.0Zn-0.2Mn-xCa (ZM-xCa, x = 0.1, 0.3, 0.5 and 1.0 wt.%) alloys in Hank’s solution was investigated with respect to phase spacing, morphology, distribution and volume fraction. With the increase in Ca addition, the volume fraction of the Ca2Mg6Zn3 phase increased from 2.5% to 7.6%, while its spacing declined monotonically from 43 μm to 30 μm. The Volta potentials of secondary phases relative to the Mg matrix were measured by using scanning kelvin probe force microscopy (SKPFM). The results show that the Volta potential of the intragranular spherical Ca2Mg6Zn3 phase (+109 mV) was higher than that of the dendritic Ca2Mg6Zn3 phase (+80 mV). It is suggested that the Ca2Mg6Zn3 acted as a cathode to accelerate the corrosion process due to the micro-galvanic effect. The corrosion preferred to occur around the spherical Ca2Mg6Zn3 phase at the early stage and developed into the intragranular region. The corrosion rate increased slightly with increasing Ca content from 0.1 wt.% to 0.5 wt.% because of the enhanced micro-galvanic corrosion effect. The decrease in the phase spacing and sharp increase in the secondary phase content resulted in a dramatic increase in the corrosion rate of the ZM-1.0Ca alloy.

1. Introduction

Magnesium (Mg) alloys have attracted great attention as promising biodegradable materials for orthopedic implants and cardiovascular interventional devices [1,2,3,4,5]. Compared with traditional metallic biomaterials, such as stainless steels and titanium alloys, Mg alloys reduce the stress-shielding risk [6]. Mg alloys usually degrade within a few weeks, and the produced Mg2+ ions can be advantageous for bone healing without toxicity [7]. However, the uncontrolled corrosion of Mg alloys may lead to unexpected mechanical failure before tissue recovery. This is a major problem for Mg alloys being used as clinical implants in a physiological environment with a high chloride and/or pH of 7.4–7.6 [7]. Therefore, controlling the corrosion of Mg alloys is becoming an urgent problem.
Alloying is one of the most effective methods to improve corrosion resistance and sustain the mechanical properties of Mg alloys [8,9]. Aluminum (Al) and rare earth elements are usually selected to modify the degradation rate of Mg alloys, but their adverse effects on biocompatibility with the human body have to be fully considered. For example, excessive Al usually causes nerve toxicity and restrains human body growth [10,11,12,13,14], while rare earth elements increase the risk of thrombosis [3]. In addition, alloying may result in precipitation of secondary phases and typically accelerate galvanic corrosion of Mg alloys, leading to the consequence of local corrosion and collapse of Mg implants. Thus, it is necessary to design and control secondary phases by choosing reasonable alloying elements, as well as heat treatments, to reduce their impacts on the corrosion rate of Mg alloys.
Manganese (Mn) is a beneficial element for improving the corrosion resistance of Mg alloys [15,16,17,18]. Studies have shown that Mn addition resulted in forming a MnO2 film on the surface of Mg alloys, inhibiting the permeation of chloride ions and improving corrosion resistance [17,18]. Zinc (Zn) is one of the most essential elements for the physiological functions of the human body [2], but Zn accelerates the corrosion rate because of forming the MgxZny phase [19,20,21]. As reported by Song [22], the MgxZny phase acted as a micro-cathode and accelerated corrosion as its volume fraction increased. Calcium (Ca) is an indispensable element of human bone, which not only accelerates bone healing [23] but also enhances corrosion resistance and mechanical performance of the implant. When Ca is added to Mg-Zn alloys, the Mg2Ca and Ca2Mg6Zn3 phases are usually formed according to the atomic ratio of Zn/Ca [24,25,26]. Although previous studies have indicated that the Ca2Mg6Zn3 phase has dominating effects on the corrosion rate of Mg-Zn-Ca alloys [27,28,29,30], its detailed corrosion behavior has not been entirely understood. In this work, we have focused on the effects of the Ca2Mg6Zn3 phase with respect to its morphology, distribution and volume fractions on the corrosion behavior of Mg-4.0Zn-0.2Mn-xCa alloys in Hank’s simulate solution, a solution similar to human body fluid, which is generally used for in vitro corrosion experiments. Its composition is given in Section 2.4. The corrosion mechanism is discussed.

2. Materials and Methods

2.1. Material Fabrication

The materials used in this work were cast in the laboratory. The as-cast Mg-4.0Zn-0.2Mn-xCa alloys (denoted as ZM-xCa alloys, x = 0.1, 0.3, 0.5 and 1.0 wt.%) were prepared using high-purity Mg (99.95 wt.%), high-purity Zn (99.99 wt.%), Mg-Mn and Mg-Ca master alloys procured from Hunan Research and Institute of Rare Earth and Material. Melting (Changsha, China) was conducted in an electrical resistance furnace under a mixed gas of N2 and SF6 (the ratio of N2 and SF6 was 100:1). The melt was kept at 750 °C for 20 min, then poured into a steel mold (preheated at 200 °C) at 720 °C and cooled to room temperature. The actual chemical compositions of the ZM-xCa alloys were examined by X-ray fluorescence (XRF, Magix-PW2403 with a test resolution of 0.0001), as shown in Table 1.

2.2. Microstructural Characterization

Microstructure observation was conducted using an optical microscope (AXIO IMAGER A2M) and a scanning electron microscope (SEM, HITACHI S3400N, HITACHI, Tokoy, Japan) equipped with energy dispersive X-ray spectroscopy (EDS). The nominal distance between secondary phases (phase spacing) and the volume fraction of precipitates were determined by Image-Pro Plus 6.0 software (Media Cybernetics, Houston, TX, USA), and 10 images were selected for data statistics at least. The samples for optical microscope observation were ground up to 5000# SiC grit papers (Federation of European Producers of Abrasives, FEPA standard) and polished with 0.5 μm diamond paste, etched by 5% HNO3/C2H6O solution for 10~20 s. X-ray diffraction (XRD, D/MAX-3C, Rigaku, Tokyo, Japan) with Cu Kα radiation was used to analyze phases with a step of 0.02° in the scanning range of 10~90° at room temperature. The microstructure features of secondary phases were characterized by transmission electron microscopy (TEM, JEM-2100, JEOL, Tokyo, Japan) equipped with an Oxford energy spectrum system (EDX can give semi-quantitative analysis, Oxford Instruments, Abingdon, UK) at an accelerating voltage of 200 kV. The dwelling time was 100 ms, and the anode voltage was 15 mV, with a current of 10 mA. Three-dimensional (3D) distribution of secondary phases was analyzed by X-ray Microscope (XRM, Xradia 520 Versa, ZEISS, Oberkochen, Baden-Württemberg, Germany) with a high effective pixel size of 1.5 μm at a voltage of 80 kV and a power of 7 W. The specimen (cylindrical shape) with dimensions of Φ1.8 mm × 25 mm was prepared for the 3D morphology test. The Object Research System (ORS) Visual software (Object Research System, Montreal, QC, Canada) was used to analyze the experimental data obtained by X-ray Microscope to reconstruct the 3D tomography image of the secondary phase.

2.3. Local Volta Potential Measurement

The potentials (relative nobility potential) of secondary phases were measured by scanning kelvin probe force microscopy (SKPFM, Bruker Icon, Bruker, Billerica, MA, USA) in the tapping mode at room temperature (~25 °C) and a relative humidity of ~50%. A magnetic etched silicon probe was used to measure the relative Volta potential, with a bias potential of 5 V applied to the sample. The tip height is 100 nm, pixel resolution is 20 nm, and scan rate is 0.5 Hz. Prior to the SKPFM test, the samples were polished with diamond paste and alcohol. The samples were vacuum packed immediately after drying with cold air. The Volta potential differences were analyzed using NanoScope Analysis 2.0 software (Bruker, Billerica, MA, USA).

2.4. In Vitro Immersion Test

The immersion test was carried out in Hank’s physiological solution (8.00 g/L NaCl, 0.40 g/L KCl, 0.14 g/L CaCl2, 0.35 g/L NaHCO3, 0.1 g/L MgCl2·6H2O, 0.06 g/L MgSO4·7H2O, 0.06 g/L KH2PO4 and 0.06 g/L Na2HPO4·12H2O, pH = 7.4) at 37 ± 0.4 °C with different periods. The samples (10 × 10 × 10 mm3) used for corrosion studies were cut from the cast block, and then ground up to 2000# SiC grit papers. Subsequently, the samples were cleaned ultrasonically with acetone and ethanol solutions, respectively. The ratio of sample surface area to solution volume was 1 cm2:150 mL and the solution was renewed every two days. After immersion, the samples for SEM were ultrasonically cleaned with 200 g/L CrO3 + 10 g/L AgNO3 solution for 10 min to remove the surface corrosion products. The average corrosion rate (estimated by weight loss, Vc) was calculated according to the following equation [31,32]:
V C = 3650   ×   ( W o   -   W t ) DAT
where, VC is the corrosion rate (mm/y), Wo is the sample weight before immersion (g), Wt is the sample weight after removing corrosion products (g), D is the density (g/cm3), A is the sample surface area exposed to the solution (cm2), and T is the immersion time (d).

2.5. Electrochemical Measurement

The samples were sealed in epoxy resin to expose only one surface (1 cm2) for electrochemical measurement. The measurement was conducted by an electrochemical workstation (Autolab, Metrohm, Herisau, Appenzell Ausserrhoden, Switzerland) with a three-electrode system, in which the saturated calomel electrode (SCE), the platinum mesh and the sample were used as reference electrode, counter electrode and working electrode, respectively. The potentiodynamic polarization tests were performed in Hank’s solution (about 200 mL) at a constant scanning rate of 0.5 mv/s, and the voltage range to open circuit potential (OCP) was ±300 mv, and the OCP monitored time was 120 s. The electrochemical parameters, such as corrosion potential (Ecorr) and corrosion current density (icorr) were obtained by Tafel extrapolation. The electrochemical impedance spectroscopy (EIS) measurement was carried out in a frequency range from 100 kHz to 100 mHz with a perturbation of 10 mV, and the EIS data (Frequency, Z’ and Z’’, about 220 data points) were fitted using ZView3.1 software (Scribner Associates, Southern Pines, NC, USA). All measurements were repeated at least three times to ensure the reproducibility of the results.

3. Results

3.1. Microstructure of ZM-xCa Alloys

Figure 1 shows the OM (a–d) and SEM (a1–d1) micrographs of the ZM-xCa alloys. As shown in Figure 1, the dendritic and spherical phases are mainly distributed along grain boundaries and within grains, respectively. Although the distribution of the secondary phases hardly changed, the grain size decreased with an increase in the Ca amount. Table 2 lists the microstructure characteristics of the ZM-xCa alloys.
This indicates that the total volume fraction of the secondary phases increased from 2.5% to 7.6%, while spacing declined from 43 μm to 30 μm when the added Ca amount increased from 0.1 wt.% to 1.0 wt.%.
Figure 2 shows the XRD patterns of the ZM-xCa alloys. Only α-Mg and Ca2Mg6Zn3 peaks are present in all ZM-xCa alloys. In addition, the diffraction intensity of the Ca2Mg6Zn3 peak increased with an increase in the Ca amount, indicating that Ca promoted the eutectic precipitation of the Ca2Mg6Zn3 phase. Figure 3 shows the TEM images and EDS results of the ZM-0.3Ca and ZM-0.5Ca alloys. The phases in these two alloys were located at grain boundaries and had a strip morphology. According to the EDS results, these secondary phases are inferred to be Ca2Mg6Zn3, showing a hexagonal crystal structure [33,34,35,36].

3.2. Electrochemical Properties of the ZM-xCa Alloys

Two typical Ca2Mg6Zn3 phases, namely the spherical (Figure 4a) and dendritic (Figure 4b) phases in the ZM-0.3Ca alloy, were chosen to conduct SKPFM analysis. The Volta potential differences between Ca2Mg6Zn3 phases and Mg matrix are revealed in Figure 4c–f.
From Figure 4c,d, it can be determined whether the spherical or the dendritic phase is brighter than the Mg matrix. The SKPFM work function mode supports the idea that the light color demonstrates more positive potential than the dark one, i.e., the light color represents the cathodic area, whereas the dark one stands for anodic one [37,38]. According to the line-profile analyses shown in Figure 4e,f, the spherical phase exhibited a relatively higher Volta potential difference (about +109 mV) than the dendritic phase (about +80 mV). These results imply that the spherical phase has a stronger acceleration effect than micro-galvanic corrosion.
The potentiodynamic polarization curves of the ZM-xCa alloys in Hank’s solution are presented in Figure 5a. The values of electrochemical parameters, i.e., corrosion potential (Ecorr), corrosion current density (icorr) and breakdown potential (Eb) are summarized in Table 3. It can be found that the Ecorr moved in the negative direction, but the icorr consistently increased with an increase in the Ca amount, and the ZM-0.1Ca alloy displayed the lowest icorr value of 5.90 × 10−7A/cm2. In the potentiodynamic polarization test, the corrosion potential is a thermodynamic parameter that reflects the probability of the corrosion tendency, while the corrosion current density is a kinetic parameter that signifies the corrosion rate [39]. The most positive corrosion potential, as well as the lowest corrosion current density of the ZM-0.1Ca alloy, indicates that it has the best corrosion resistant property. Moreover, the ZM-0.1Ca alloy has the most positive breakdown potential (Eb) of −1.450 V, which indicates that the corrosion reaction is more difficult to proceed because of the formed corrosion film [40].
Figure 5b–d indicates the EIS results of the ZM-xCa alloys. As shown in Figure 5b, the Nyquist plots of the four alloys are composed of capacitance loops at high frequency and an inductive loop at low frequency. All of the Nyquist plots are similar in shape except for the diameter of the loop. This result demonstrates that the corrosion mechanism of the four alloys is similar, but their corrosion rates are different. According to the Nyquist plots, the corrosion rate ranks as ZM-0.1Ca ˂ ZM-0.3Ca ˂ ZM-0.5Ca ˂ ZM-1.0Ca. In addition, the inductive loop at a low frequency implies a breakdown of the protective corrosion-products film [41]. Figure 5c shows the impedance modulus (|Z|), as well as the Bode phase angle plots of the ZM-xCa alloys. The largest impedance modulus (|Z|) of the ZM-0.1Ca alloy represents the best corrosion protection resulting from the corrosion-product film. The maximum crest of the Bode phase angle plot also reflects the difficulty of charge transfer of the ZM-0.1Ca alloy. Figure 5d indicates the fitted equivalent circuit using the EIS data. Rs, Rf and Rct are solution resistance, film resistance and charge transfer resistance, respectively. CPE1 represents the constant phase element of corrosion product film, CPE2 represents the double layer capacitance. L and RL are the inductance and inductance resistance. The detailed fitting results are listed in Table 4.
The polarization resistance (Rp), which is inversely proportional to the corrosion rate, is an important parameter for evaluating the corrosion performance of an alloy. Its value was calculated using the following equation:
R P = R S   + R f + R ct R L R ct + R L
The calculated Rp of the ZM-xCa alloys is also listed in Table 4. The largest Rp of the ZM-0.1Ca alloy demonstrated its best corrosion resistance, which is consistent with the polarization result.

3.3. Corrosion Behaviors of ZM-xCa Alloys

Figure 6 shows the corrosion rates of the ZM-xCa alloys by weight loss after immersion in Hank’s solution for 7 days and 14 days, respectively.
The corrosion rate increases with an increase in the added Ca amount for neither 7-day nor 14-day immersion. The corrosion rate increased slowly when the added Ca amount was less than 0.5 wt.%; however, it sharply increased for the ZM-1.0Ca alloy. In particular, the 14-day corrosion rate of the ZM-1.0Ca alloy is about three times that of the ZM-0.1Ca alloy. These results demonstrate that excessive Ca addition destructs the corrosion resistance of the ZM-xCa alloys.
The surface morphologies after removal of corrosion products of the ZM-xCa alloys with various immersion times are displayed in Figure 7. After 7-day immersion, a shallow corrosion area extended with an increase in the added Ca amount, as shown in Figure 7a–c,e. On the other hand, corrosion morphology also changes significantly with corrosion time. In the case of the ZM-1.0Ca alloy, plenty of tiny corrosion pits appeared after 3-day immersion (Figure 7d), and an almost whole corroded morphology was presented after 7-day immersion (Figure 7e). The corrosion pits became corrosion cavities with an extension of the corrosion time. The corrosion cavity became deeper and wider and reached about 554 μm after 14-day immersion (Figure 7d1–f1).

4. Discussion

The Ca2Mg6Zn3 phase plays a significant role in the corrosion process of magnesium alloys [42,43]. In the present study, the corrosion behavior of the ZM-xCa alloys is investigated by altering the Ca2Mg6Zn3 phase morphology, distribution and volume fraction. Figure 8 shows the 3D topographical characteristics of the Ca2Mg6Zn3 phase in the ZM-0.3Ca alloy, giving an intuitive distribution of the secondary phase. It was found that there are two kinds of morphologies of the Ca2Mg6Zn3 phase, one spherical and the other dendritic. In addition, the dendritic (marked with red color) Ca2Mg6Zn3 phase precipitated at grain boundaries and connected with each other, forming a continuous network, while the spherical (marked with violet color) Ca2Mg6Zn3 phase was distributed within grains. These results are consistent with the optical images shown in Figure 1.
The Volta potential in air is widely used in the corrosion field to assess the corrosion tendency of Mg alloys [42,43,44]. According to the SKPFM results shown in Figure 4, the Volta potential of either the dendritic or the spherical Ca2Mg6Zn3 phase is higher than that of the Mg matrix; hence, not only the dendritic but also the spherical Ca2Mg6Zn3 phase acts as a cathode, while the Mg matrix acts as an anode in micro-galvanic corrosion. As a result, the Mg matrix dissolves preferentially during the immersion period. Therefore, the total amount of the Ca2Mg6Zn3 phase, as well as its phase spacing, plays a controlling role in the corrosion process; that is, the higher the volume fraction and/or the smaller the phase spacing, the higher the corrosion rate. Figure 9 shows the relationship between the corrosion rate, the volume fraction and the spacing of the secondary phase in the ZM-xCa alloys. With the increase in the volume fraction and decrease in the spacing of the secondary phase, the corrosion rate of the ZM-xCa alloys after 14-day immersion increases. The increase in the total secondary phase creates more micro-galvanic positions, and the shortening phase spacing decreases the distance between the corrosion pits. These two aspects simultaneously promoted the corrosion rate of the ZM-xCa alloys.
Because the SKPFM results show that the Volta potential of the spherical Ca2Mg6Zn3 phase is higher than that of the dendritic one, the spherical phase is electrochemically preferred as a cathode to accelerate Mg matrix (anode) dissolution in the micro-galvanic couple.
We discussed the ion exchange process and formation of the corrosion products during the corrosion process of Mg alloy in our previous studies [3,31]. We do not discuss this in the present investigation. The present research focuses on the effect of secondary phase characteristics on the corrosion behavior of Mg alloys. Figure 10 intuitively illustrates a schematic view of the corrosion behavior of the ZM-0.1Ca and ZM-1.0 alloys. The corrosion process occurs preferentially around spherical phases in stage I (as shown in Figure 10a,d). Because of the dissolution of the Mg matrix around the spherical phase, it falls off and forms corrosion pits in stage II. If the phase spacing is large, for example, in the ZM-0.1Ca alloy, the corrosion process is difficult to proceed to another phase; hence, small corrosion pits are formed (as shown in Figure 10b). As immersion continues, the corrosion process proceeds into grains, and the corrosion process occurs around the dendritic phase distributing at grain boundaries. This corrosion is different from that in grains. Instead of forming corrosion pits, a corrosion “channel” along the dendritic phase is formed, which induces the corrosion process to proceed into the interior grains, as shown in Figure 10b,d. For the alloy with a high Ca content, corrosion penetrates speedily and continuously along grain boundaries. Because of falling off these dendritic phases and dissolution of grains, large corrosion cavities are formed in stage III (see Figure 10f), resulting in a rapid corrosion rate. However, in the case of Zn-0.1Ca alloy, the corrosion pits caused by pitting corrosion are difficult to connect; hence, independent small-scale corrosion pits are generated in the Zn-0.1Ca alloy (as shown in Figure 10c), resulting in slow mass loss.

5. Conclusions

  • The cast ZM-xCa (0.1, 0.3, 0.5 and 1.0 wt.%) alloys contain the intragranular spherical Ca2Mg6Zn3 phase and the dendritic one at grain boundaries. The volume fraction of the Ca2Mg6Zn3 phase gradually increased from 2.5% to 7.6%, while its spacing declined monotonically from 43.0 μm to 30.0 μm with an increase in the added Ca amount from 0.1 wt.% to 1.0 wt.%.
  • The Volta potential of the spherical Ca2Mg6Zn3 phase (+109 mV) was higher than that of the dendritic phase (+80 mV); hence, the spherical phase was electrochemically preferred as a cathode to accelerate Mg matrix (anode) dissolution in the micro-galvanic couple.
  • The corrosion rate obtained by weight loss increased slightly with increasing Ca content from 0.1 wt.% to 0.5 wt.% because of the enhanced micro-galvanic corrosion effect. The decrease in the phase spacing and sharp increase in the secondary phase content resulted in a dramatic increase in the corrosion rate of the ZM-1.0Ca alloy.

Author Contributions

Conceptualization, J.F. and W.D.; methodology, J.F. and W.D.; software, J.F.; validation, W.D., K.L. and H.L.; formal analysis, J.F. and S.L.; investigation, J.F., A.M. and X.D.; resources, C.Z. and Z.W.; J.F. data curation; J.F. writing—original draft preparation; W.D., K.L. and H.L. writing—review and editing. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the Beijing Natural Science Foundation (No. 2192006) and the National Natural Science Foundation of China (No. 51801004; No. 52001015).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

All data are available within the manuscript.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Birbilis, N.; Easton, M.A.; Sudholz, A.D.; Zhu, S.M.; Gibson, M.A. On the corrosion of binary magnesium-rate earth alloys. Corros. Sci. 2009, 51, 683–689. [Google Scholar] [CrossRef]
  2. Zhang, S.X.; Zhang, X.N.; Zhao, C.L.; Li, J.N.; Song, Y.; Xie, C.Y.; Tao, H.R.; Zhang, Y.; He, Y.H.; Jiang, Y.; et al. Research on an Mg–Zn alloy as a degradable biomaterial. Acta Biomater. 2010, 6, 626–640. [Google Scholar] [CrossRef]
  3. Du, W.B.; Liu, K.; Ma, K.; Wang, Z.H.; Li, S.B. Effects of trace Ca/Sn addition on corrosion behaviors of biodegradable Mg–4Zn–0.2Mn alloy. J. Magnes. Alloy 2018, 6, 1–14. [Google Scholar] [CrossRef]
  4. Munir, K.; Lin, J.X.; Wen, C.E.; Wright, P.F.A.; Li, Y.C. Mechanical, corrosion, and biocompatibility properties of Mg-Zr-Sr-Sc alloys for biodegradable implant applications. Acta Biomater. 2020, 102, 493–507. [Google Scholar] [CrossRef]
  5. Witte, F. The history of biodegradable magnesium implants. Acta Biomater. 2010, 6, 1680–1692. [Google Scholar] [CrossRef]
  6. Lu, Y.; Bradshaw, A.R.; Chiu, Y.L.; Jones, I.P. Effects of secondary phase and grain size on the corrosion of biodegradable Mg-Zn-Ca alloys. Mater. Sci. Eng. C 2015, 48, 480–486. [Google Scholar] [CrossRef]
  7. Witte, F.; Kaese, V.; Haferkamp, H.; Switzer, E.; Meyer-Lingenberg, A.; Wirth, C.J.; Windhagen, H. In vivo corrosion of four magnesium alloys and the associated bone response. Biomaterials 2005, 26, 3557–3563. [Google Scholar] [CrossRef] [PubMed]
  8. Zhao, M.C.; Liu, M.; Song, G.L.; Atrens, A. Influence of the β-phase morphology on the corrosion of the Mg alloy AZ91. Corros. Sci. 2008, 50, 1939–1953. [Google Scholar] [CrossRef]
  9. Atrens, A.; Song, G.L.; Liu, M.; Shi, Z.M.; Cao, F.Y.; Dargusch, M.S. Review of recent developments in the field of magnesium corrosion. Adv. Eng. Mater. 2015, 17, 400–453. [Google Scholar] [CrossRef]
  10. Cai, C.H.; Alvens, M.M.; Song, R.B.; Wang, Y.J.; Li, J.Y.; Montemor, M.F. Non-destructive corrosion study on a magnesium alloy with mechanical properties tailored for biodegradable cardiovascular stent applications. J. Mater. Sci. Technol. 2021, 66, 128–138. [Google Scholar] [CrossRef]
  11. Zengin, H.; Turen, Y. Effect of Y addition on microstructure and corrosion behavior of extruded Mg–Zn–Nd–Zr alloy. J. Magnes. Alloy 2020, 8, 640–653. [Google Scholar] [CrossRef]
  12. Jin, S.; Zhang, D.; Lu, X.P.; Zhang, Y.; Tan, L.L.; Liu, Y.; Wang, Q. Mechanical properties, biodegradability and cytocompatibility of biodegradable Mg-Zn-Zr-Nd/Y alloys. J. Mater. Sci. Technol. 2020, 47, 190–201. [Google Scholar] [CrossRef]
  13. Zhang, E.L.; Yang, L. Microstructure, mechanical properties and bio-corrosion properties of Mg-Zn-Mn-Ca alloy for biomedical application. Mater. Sci. Eng. A 2008, 497, 111–118. [Google Scholar] [CrossRef]
  14. Ding, Y.F.; Wen, C.E.; Hodgson, P.; Li, Y.C. Effects of alloying elements on the corrosion behavior and biocompatibility of biodegradable magnesium alloys: A review. J. Mater. Chem. B 2014, 2, 1912–1933. [Google Scholar] [CrossRef] [PubMed]
  15. Metalnikov, P.; Ben-Hamu, G.; Templeman, Y.; Shin, K.S.; Meshi, L. The relation between Mn additions, microstructure and corrosion behavior of new wrought Mg-5Al alloys. Mater. Charact. 2018, 145, 101–115. [Google Scholar] [CrossRef]
  16. Wang, J.F.; Huang, S.; Li, Y.; Wei, Y.Y.; Xi, X.F.; Cai, K.Y. Microstructure, mechanical and bio-corrosion properties of Mn-doped Mg–Zn–Ca bulk metallic glass composites. Mater. Sci. Eng. C 2013, 33, 3832–3838. [Google Scholar] [CrossRef]
  17. Cho, D.H.; Lee, B.W.; Park, J.Y.; Cho, K.M.; Park, I.M. Effect of Mn addition on corrosion properties of biodegradable Mg-4Zn-0.5Ca-xMn alloys. J. Alloys Compd. 2017, 695, 1166–1174. [Google Scholar] [CrossRef]
  18. Bazhenov, V.E.; Li, A.V.; Komissarov, A.A.; Koltygin, A.V.; Tavolzhanskii, S.A.; Bautin, V.A.; Voropaeva, O.O.; Mukhametshina, A.M.; Tokar, A.A. Microstructure and mechanical and corrosion properties of hot-extruded Mg-Zn-Ca-(Mn) biodegradable alloys. J. Magnes. Alloy 2020, 9, 1428–1442. [Google Scholar] [CrossRef]
  19. Cai, S.H.; Lei, T.; Li, N.F.; Feng, F.F. Effects of Zn on microstructure, mechanical properties and corrosion behavior of Mg-Zn alloys. Mater. Sci. Eng. C 2012, 32, 2570–2577. [Google Scholar] [CrossRef]
  20. Li, H.; Peng, Q.M.; Li, X.J.; Li, K.; Han, Z.S.; Fang, D.Q. Microstructures, mechanical and cytocompatibility of degradable Mg-Zn based orthopedic biomaterials. Mater. Des. 2014, 58, 43–51. [Google Scholar] [CrossRef]
  21. Zhang, E.L.; Yang, L.; Xu, J.W.; Chen, H.Y. Microstructure, mechanical properties and bio-corrosion properties of Mg-Si(-Ca, Zn) alloy for biomedical application. Acta Biomater. 2010, 6, 1756–1762. [Google Scholar] [CrossRef]
  22. Song, Y.W.; Han, E.H.; Shan, D.Y.; Yim, C.D.; You, B.Y. The effect of Zn concentration on the corrosion behavior of Mg-xZn alloys. Corros. Sci. 2012, 65, 322–330. [Google Scholar] [CrossRef]
  23. Zander, D.; Zumdick, N.A. Influence of Ca and Zn on the microstructure and corrosion of biodegradable Mg–Ca–Zn alloys. Corros. Sci. 2015, 93, 222–233. [Google Scholar] [CrossRef]
  24. Erdmann, N.; Angrisani, N.; Reifenrath, J.; Lucas, A.; Thorey, F.; Bormann, D.; Meyer-Lindenberg, A. Biomechanical testing and degradation analysis of MgCa0.8 alloy screws: A comparative in vivo study in rabbits. Acta Biomater. 2011, 7, 1421–1428. [Google Scholar] [CrossRef]
  25. Li, Z.J.; Gu, X.N.; Lou, S.Q.; Zheng, Y.F. The development of binary Mg-Ca alloys for use as biodegradable materials within bone. Biomaterials 2008, 29, 1329–1344. [Google Scholar] [CrossRef] [PubMed]
  26. Kim, W.C.; Kim, J.G.; Lee, J.Y.; Seok, H.K. Influence of Ca on the corrosion properties of magnesium for biomaterials. Mater. Lett. 2008, 62, 4146–4148. [Google Scholar] [CrossRef]
  27. Bakhsheshi-Rad, H.R.; Abdul-Kadir, M.R.; Idris, M.H.; Farahany, S. Relationship between the corrosion behavior and the thermal characteristics and microstructure of Mg-0.5Ca-xZn alloys. Corros. Sci. 2012, 64, 184–197. [Google Scholar] [CrossRef] [Green Version]
  28. Asadi, J.; Korojy, B.; Hosseini, A.; Alishahi, M. Effect of cell structure on mechanical and bio-corrosion behavior of biodegradable Mg-Zn-Ca foam. Mater. Today Commun. 2021, 28, 102715. [Google Scholar] [CrossRef]
  29. Gong, C.W.; He, X.Z.; Fang, D.Q.; Liu, B.S.; Yan, X. Effect of second phases on discharge properties and corrosion behaviors of the Mg-Ca-Zn anodes for primary Mg-air batteries. J. Alloys Compd. 2021, 861, 158493. [Google Scholar] [CrossRef]
  30. Meng, X.; Jiang, Z.T.; Zhu, S.J.; Guan, S.K. Effects of Sr addition on microstructure, mechanical and corrosion properties of biodegradable Mg–Zn–Ca alloy. J. Alloys Compd. 2020, 838, 155611. [Google Scholar] [CrossRef]
  31. Cheng, Y.F.; Du, W.B.; Liu, K.; Fu, J.J.; Wang, Z.H.; Li, S.B.; Fu, J.L. Mechanical properties and corrosion behaviors of Mg-4Zn-0.2Mn-0.2Ca alloy after long term in vitro degradation. Trans. Nonferrous Met. Soc. China 2020, 30, 363–372. [Google Scholar] [CrossRef]
  32. Liu, J.; Yang, L.X.; Zhang, C.Y.; Zhang, B.; Zhang, T.; Li, Y.; Wu, K.M.; Wang, F.H. Significantly improved corrosion resistance of Mg-15Gd-2Zn-0.39Zr alloys: Effect of heat-treatment. J. Mater. Sci. Technol. 2019, 35, 1644–1654. [Google Scholar] [CrossRef]
  33. Duley, P.; Sanyal, S.; Bandyopadhyay, T.K.; Mandal, S. Homogenization-induced age-hardening behavior and room temperature mechanical properties of Mg-4Zn-0.5Ca-0.16Mn (wt%) alloy. Mater. Des. 2019, 164, 107554. [Google Scholar] [CrossRef]
  34. Zhang, Y.; Li, J.X.; Li, J.Y. Effects of calcium addition on phase characteristics and corrosion behaviors of Mg-2Zn-0.2Mn-xCa in simulated body fluid. J. Alloys Compd. 2017, 728, 37–46. [Google Scholar] [CrossRef]
  35. Jiang, M.G.; Xu, C.; Nakata, T.; Yan, H.; Chen, R.S.; Kamado, S. Development of dilute Mg-Zn-Ca-Mn alloy with high performance via extrusion. J. Alloys Compd. 2016, 668, 13–21. [Google Scholar] [CrossRef]
  36. Liu, C.Q.; Chen, X.H.; Chen, J.; Atrens, A.; Pan, F.S. The effects of Ca and Mn on the microstructure, texture and mechanical properties of Mg-4Zn alloy. J. Magnes. Alloy. 2020, 9, 1084–1097. [Google Scholar] [CrossRef]
  37. Liu, J.H.; Song, Y.W.; Chen, J.C.; Chen, P.; Shan, D.Y.; Han, E.H. The Special Role of Anodic Second Phases in the Micro-galvanic Corrosion of EW75 Mg Alloy. Electrochim. Acta 2016, 189, 190–195. [Google Scholar] [CrossRef]
  38. Cai, C.H.; Song, R.B.; Wang, L.X.; Li, J.Y. Effect of anodic T phase on surface micro-galvanic corrosion of biodegradable Mg-Zn-Zr-Nd alloys. Appl. Surf. Sci. 2018, 462, 243–254. [Google Scholar] [CrossRef]
  39. Gui, Z.Z.; Kang, Z.X.; Li, Y.Y. Corrosion mechanism of the as-cast and as-extruded biodegradable Mg-3.0Gd-2.7Zn-0.4Zr-0.1Mn alloys. Mater. Sci. Eng. C 2019, 96, 831–840. [Google Scholar] [CrossRef]
  40. Zhang, T.; Meng, G.Z.; Shao, Y.W.; Cui, Z.Y.; Wang, F.H. Corrosion of hot extrusion AZ91 magnesium alloy. Part II: Effect of rare earth element neodymium (Nd) on the corrosion behavior of extruded alloy. Corros. Sci. 2011, 53, 2934–2942. [Google Scholar] [CrossRef]
  41. Bakhsheshi-Rad, H.R.; Idris, M.H.; Abdul-Kadir, M.R.; Ourdjini, A.; Medraj, M.; Daroonparvar, M.; Hamzah, E. Mechanical and bio-corrosion properties of quaternary Mg–Ca–Mn–Zn alloys compared with binary Mg–Ca alloys. Mater. Des. 2014, 53, 283–292. [Google Scholar] [CrossRef]
  42. Pan, H.; Pang, K.; Cui, F.Z.; Ge, F.; Man, C.; Wang, X.; Cui, Z.Y. Effect of alloyed Sr on the microstructure and corrosion behavior of biodegradable Mg-Zn-Mn alloy in Hanks’ solution. Corros. Sci. 2019, 157, 420–437. [Google Scholar] [CrossRef]
  43. Yin, S.Q.; Duan, W.C.; Liu, W.H.; Wu, L.; Yu, J.M.; Zhao, Z.L.; Liu, M.; Wang, P.; Cui, J.Z.; Zhang, Z.Q. Influence of specific second phases on corrosion behaviors of Mg-Zn-Gd-Zr alloys. Corros. Sci. 2020, 166, 108419. [Google Scholar] [CrossRef]
  44. Wei, L.Y.; Li, J.Y.; Zhang, Y.; Lai, H.Y. Effects of Zn content on microstructure, mechanical and degradation behaviors of Mg-xZn-0.2Ca-0.1Mn alloys. Mater. Chem. Phys. 2020, 241, 122441. [Google Scholar] [CrossRef]
Figure 1. OM (ad) and SEM (a1d1) micrographs of the as-cast ZM-0.1Ca (a,a1), ZM-0.3Ca (b,b1), ZM-0.5Ca (c,c1) and ZM-1.0Ca (d,d1) alloys.
Figure 1. OM (ad) and SEM (a1d1) micrographs of the as-cast ZM-0.1Ca (a,a1), ZM-0.3Ca (b,b1), ZM-0.5Ca (c,c1) and ZM-1.0Ca (d,d1) alloys.
Materials 15 02079 g001
Figure 2. XRD patterns of ZM-xCa alloys: (a) ZM-0.1Ca, (b) ZM-0.3Ca, (c) ZM-0.5Ca and (d) ZM-1.0Ca.
Figure 2. XRD patterns of ZM-xCa alloys: (a) ZM-0.1Ca, (b) ZM-0.3Ca, (c) ZM-0.5Ca and (d) ZM-1.0Ca.
Materials 15 02079 g002
Figure 3. TEM images and EDS results of the secondary phases: (a,b) ZM-0.3Ca and (c,d) ZM-0.5Ca alloys.
Figure 3. TEM images and EDS results of the secondary phases: (a,b) ZM-0.3Ca and (c,d) ZM-0.5Ca alloys.
Materials 15 02079 g003
Figure 4. SEM images and SKPFM analysis of the ZM-0.3Ca alloy: (a) SEM images of the spherical secondary phase and (b) the dendritic secondary phase; (c) SKPFM maps of the spherical secondary phase and (d) the dendritic secondary phase; (e) the Volta potential profile of line as indicated in (c); (f) the Volta potential profile of line as indicated in (d).
Figure 4. SEM images and SKPFM analysis of the ZM-0.3Ca alloy: (a) SEM images of the spherical secondary phase and (b) the dendritic secondary phase; (c) SKPFM maps of the spherical secondary phase and (d) the dendritic secondary phase; (e) the Volta potential profile of line as indicated in (c); (f) the Volta potential profile of line as indicated in (d).
Materials 15 02079 g004
Figure 5. Potentiodynamic polarization curves (a) and electrochemical impedance spectra of the ZM-xCa alloys: (b) Nyquist plots, (c) Bode impedance and Bode phase angle plots, and (d) Equivalent circuit.
Figure 5. Potentiodynamic polarization curves (a) and electrochemical impedance spectra of the ZM-xCa alloys: (b) Nyquist plots, (c) Bode impedance and Bode phase angle plots, and (d) Equivalent circuit.
Materials 15 02079 g005
Figure 6. Corrosion rates of the ZM-xCa alloys obtained by weight loss after immersion in Hank’s solution for different times.
Figure 6. Corrosion rates of the ZM-xCa alloys obtained by weight loss after immersion in Hank’s solution for different times.
Materials 15 02079 g006
Figure 7. Surface morphologies after removal of the corrosion products with various immersion times in Hank’s solution of the ZM-xCa alloys: (ac) ZM-0.1Ca, ZM-0.3Ca and ZM-0.5Ca alloys immersed for 7-day; (d,d1), (e,e1) and (f,f1) ZM-1.0Ca alloy immersed for 3-day, 7-day and 14-day, respectively.
Figure 7. Surface morphologies after removal of the corrosion products with various immersion times in Hank’s solution of the ZM-xCa alloys: (ac) ZM-0.1Ca, ZM-0.3Ca and ZM-0.5Ca alloys immersed for 7-day; (d,d1), (e,e1) and (f,f1) ZM-1.0Ca alloy immersed for 3-day, 7-day and 14-day, respectively.
Materials 15 02079 g007
Figure 8. Three-dimensional topographical characteristics of the Ca2Mg6Zn3 secondary phase in the ZM-0.3Ca alloy: (a) perspective view, (b) sectional view of the perpendicular Y axle.
Figure 8. Three-dimensional topographical characteristics of the Ca2Mg6Zn3 secondary phase in the ZM-0.3Ca alloy: (a) perspective view, (b) sectional view of the perpendicular Y axle.
Materials 15 02079 g008
Figure 9. Relationship between corrosion rate, secondary phase spacing and volume fraction of the ZM-xCa alloys.
Figure 9. Relationship between corrosion rate, secondary phase spacing and volume fraction of the ZM-xCa alloys.
Materials 15 02079 g009
Figure 10. Schematic illustration of corrosion process of the investigated alloys in Hank’s solution: (ac) ZM-0.1Ca alloy and (df) ZM-1.0Ca alloy.
Figure 10. Schematic illustration of corrosion process of the investigated alloys in Hank’s solution: (ac) ZM-0.1Ca alloy and (df) ZM-1.0Ca alloy.
Materials 15 02079 g010
Table 1. Actual compositions of the ZM-xCa alloys (wt.%).
Table 1. Actual compositions of the ZM-xCa alloys (wt.%).
AlloysActual Compositions (wt.%)
ZnMnCaSiMg
ZM-0.1Ca4.130.200.12<0.02Bal.
ZM-0.3Ca3.810.170.34<0.02Bal.
ZM-0.5Ca3.780.180.56<0.03Bal.
ZM-1.0Ca3.760.180.95<0.02Bal.
Table 2. Microstructure characteristics of the ZM-xCa alloys (wt.%).
Table 2. Microstructure characteristics of the ZM-xCa alloys (wt.%).
AlloysVolume Fraction of Secondary Phase (%)Secondary Phase Spacing (μm)
ZM-0.1Ca2.5 ± 0.243.4 ± 2.0
ZM-0.3Ca3.0 ± 0.239.3 ± 2.1
ZM-0.5Ca4.2 ± 0.332.5 ± 1.5
ZM-1.0Ca7.6 ± 0.430.1 ± 1.2
Table 3. Electrochemical parameters of the ZM-xCa alloys.
Table 3. Electrochemical parameters of the ZM-xCa alloys.
AlloysEcorr (V)icorr (A/cm2)Eb (V)
ZM-0.1Ca−1.5305.90 × 10−7−1.450
ZM-0.3Ca−1.5756.63 × 10−7−1.524
ZM-0.5Ca−1.6176.77 × 10−7−1.527
ZM-1.0Ca−1.6621.31 × 10−6−1.542
Table 4. The fitting results of the EIS spectra of ZM-xCa alloys.
Table 4. The fitting results of the EIS spectra of ZM-xCa alloys.
AlloysRs
(Ω cm2)
Rf
(Ω cm2)
CPE1
(10–6 F/cm2)
n1CPE2
(10–6 F/cm2)
n2Rct
(kΩ cm2)
RL
(kΩ cm2)
L
(H cm2)
RP
(kΩ cm2)
ZM-0.1Ca25.48281.317.600.736.310.9031.2953.972.26 × 10620.11
ZM-0.3Ca22.41278.439.130.706.660.8925.1770.051.61 × 10618.80
ZM-0.5Ca22.40230.2111.710.698.830.8545.6920.251.12 × 10614.28
ZM-1.0Ca21.57206.3019.080.665.160.8810.8016.902.30 × 1066.86
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Fu, J.; Du, W.; Liu, K.; Du, X.; Zhao, C.; Liang, H.; Mansoor, A.; Li, S.; Wang, Z. Effect of the Ca2Mg6Zn3 Phase on the Corrosion Behavior of Biodegradable Mg-4.0Zn-0.2Mn-xCa Alloys in Hank’s Solution. Materials 2022, 15, 2079. https://doi.org/10.3390/ma15062079

AMA Style

Fu J, Du W, Liu K, Du X, Zhao C, Liang H, Mansoor A, Li S, Wang Z. Effect of the Ca2Mg6Zn3 Phase on the Corrosion Behavior of Biodegradable Mg-4.0Zn-0.2Mn-xCa Alloys in Hank’s Solution. Materials. 2022; 15(6):2079. https://doi.org/10.3390/ma15062079

Chicago/Turabian Style

Fu, Junjian, Wenbo Du, Ke Liu, Xian Du, Chenchen Zhao, Hongxing Liang, Adil Mansoor, Shubo Li, and Zhaohui Wang. 2022. "Effect of the Ca2Mg6Zn3 Phase on the Corrosion Behavior of Biodegradable Mg-4.0Zn-0.2Mn-xCa Alloys in Hank’s Solution" Materials 15, no. 6: 2079. https://doi.org/10.3390/ma15062079

APA Style

Fu, J., Du, W., Liu, K., Du, X., Zhao, C., Liang, H., Mansoor, A., Li, S., & Wang, Z. (2022). Effect of the Ca2Mg6Zn3 Phase on the Corrosion Behavior of Biodegradable Mg-4.0Zn-0.2Mn-xCa Alloys in Hank’s Solution. Materials, 15(6), 2079. https://doi.org/10.3390/ma15062079

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop