Next Article in Journal
A Review of Particle Size Analysis with X-ray CT
Previous Article in Journal
Compression Behavior of Concrete Columns Strengthened with Fiber-Reinforced Inorganic Composites Based on Magnesium Phosphate Cement
Previous Article in Special Issue
Superfunctional Materials by Ultra-Severe Plastic Deformation
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Can Severe Plastic Deformation Tune Nanocrystallization in Fe-Based Metallic Glasses?

1
Erich Schmid Institute of Materials Science, Austrian Academy of Sciences, 8700 Leoben, Austria
2
Department of Materials Science, Chair of Materials Physics, Montanuniversität Leoben, 8700 Leoben, Austria
3
Department of Mechanical Engineering, University of Dunaujvaros, 2400 Dunaujvaros, Hungary
4
Vacuumschmelze GmbH & Co. KG (VAC) Rapid Solidification Technology, 63450 Hanau, Germany
5
Research Group Physics of Nanostructured Materials, Faculty of Physics, University of Vienna, 1090 Wien, Austria
*
Author to whom correspondence should be addressed.
Materials 2023, 16(3), 1260; https://doi.org/10.3390/ma16031260
Submission received: 23 December 2022 / Revised: 20 January 2023 / Accepted: 26 January 2023 / Published: 1 February 2023
(This article belongs to the Special Issue Metallurgy by Severe Plastic Deformation)

Abstract

:
The effects of severe plastic deformation (SPD) by means of high-pressure torsion (HPT) on the structural properties of the two iron-based metallic glasses Fe73.9Cu1Nb3Si15.5B6.6 and Fe81.2Co4Si0.5B9.5P4Cu0.8 have been investigated and compared. While for Fe73.9Cu1Nb3Si15.5B6.6, HPT processing allows us to extend the known consolidation and deformation ranges, HPT processing of Fe81.2Co4Si0.5B9.5P4Cu0.8 for the first time ever achieves consolidation and deformation with a minimum number of cracks. Using numerous analyses such as X-ray diffraction, dynamic mechanical analyses, and differential scanning calorimetry, as well as optical and transmission electron microscopy, clearly reveals that Fe81.2Co4Si0.5B9.5P4Cu0.8 exhibits HPT-induced crystallization phenomena, while Fe73.9Cu1Nb3Si15.5B6.6 does not crystallize even at the highest HPT-deformation degrees applied. The reasons for these findings are discussed in terms of differences in the deformation energies expended, and the number and composition of the individual crystalline phases formed. The results appear promising for obtaining improved magnetic properties of glassy alloys without additional thermal treatment.

1. Introduction

In recent times, it has become increasingly important to focus on ways to consume electric energy more efficiently. As magnetic losses—proportional to the area of the B-H-loop—play a significant role in energy consumption (e.g., [1]), it is vital to gain a better understanding of how they can be controlled. Already 40 years ago, it has been found that Fe-based metallic glasses are highly efficient soft magnetic alloys (e.g., [2,3]), especially with respect to achieving low coercivity. Since then, further efforts have been undertaken to improve the magnetic and mechanical properties of such alloys and to establish synthesis routes allowing for larger materials dimensions (e.g., [4,5,6,7,8,9]). The latter is most important, as upscaling melt-spun tapes (thickness of only ~20 µm) would extend their applicability to, e.g., electric engines, and could thereby contribute to a greener future by globally reducing the CO2 footprint of electrical devices.
To tune the magnetic properties of these alloys, annealing in an external magnetic field and under external stress is applied (e.g., [6,10,11,12]). Thereby, crystallization of α-Fe und Fe3Si [13] from the amorphous phase is induced, which increases the otherwise rather limited saturation polarization (e.g., [3]).
Following the group of Aronin [14], plastic deformation—at best the various methods of SPD (Severe Plastic Deformation) because of the suppression of cracks by the enhanced hydrostatic pressure component (e.g., [15,16])—can provide sufficient structural inhomogeneities as nuclei for controlled nanocrystallization due to a competition of homogeneous deformation and shear banding [17]. Recent results indicate that the hydrostatic pressure during HPT (e.g., [15,18]) may induce local ordering during the deformation process [19] which could further ease the nucleation in some alloy systems.
The most prominent candidate among soft magnetic Fe-based metallic glasses is Finemet/Vitroperm (tradenames Hitachi and VAC, respectively). This material with composition Fe73.5Cu1Nb3Si13.5B9 is available as thin amorphous ribbons which become nanocrystalline (although brittle) after heat treatment (at approximately 510 °C (783 K)). In this alloy, the elements Cu and Nb play a major role in the nanocrystallization process [20].
If deformation-induced nanocrystallization could be achieved, one could resign on Cu and Nb additions, rendering a higher amount of Fe for providing a high magnetization while nanocrystals—with sizes smaller than 50 nm—still achieve a low coercivity [21]. Indeed, the Aronin group [14] reached a high saturation polarization although the coercivity was considerable. The latter may be reduced by adequate heat treatment [22]. As SPD has some potential for amorphization, also the non-magnetic additives Si and B could be omitted, again increasing the percentage of Fe and thus increasing the low saturation polarization of 1.4 T, thereby making the material more attractive for commercial applications. Makino et al. [23] showed that additions of P and Co—thus providing alloys like Fe83.3–84.3Si4B8P3–4Cu0.7 and Fe81.2Co4Si0.5B9.5P4Cu0.8, achieve a saturation polarization of 1.88–1.94 T, but so far these alloys were not produced with the appropriate nanosized microstructure. Therefore, applying SPD processing appears as a very promising route to reach nanocrystallinity, providing low coercivity and high saturation polarization at the same time.
Because of the very high hardness of the Vitroperm alloy Fe73.9Cu1Nb3Si15.5B6.6 (6–10 GPa) and particularly of Makino’s alloy Fe81.2Co4Si0.5B9.5P4Cu0.8 (up to 16 GPa at least when fully crystallized), the feature of SPD methods utilizing high hydrostatic pressures up to about 10 GPa seems essential to provide any plastic deformation in these alloys (e.g., [5,24,25,26]). So far, some amount of deformation has been achieved by ball milling [27], impact hammering [28]) and HPT (e.g., [14,29,30,31]) but these efforts were so far limited to very small samples. However, SPD methods are basically bottom-up methods to achieve bulk nanocrystalline and/or amorphous metals and alloys, they are not only capable of nanocrystallization but can even realize massive materials from amorphous ribbons (e.g., [15]).
In a recent work [32] we proved this for the example of Vitroperm Fe73.9Cu1Nb3Si15.5B6.6 applying HPT with pressures of 7.5 GPa using deformation temperatures Tdef = 473, 573, and 673 K for one turn. In the present paper, we report on further investigations of HPT effects applied on this glass but also present results on the ‘Makino’-type alloy Fe81.2Co4Si0.5B9.5P4Cu0.8 because of the motivation given above. Of special interest is the question of whether the application of HPT provides some nanocrystallization thus allowing for the replacement of Cu and Nb and/or for some further thermal treatment, to finally achieve an excellent soft magnetic material with maximum saturation polarization and minimum coercivity.

2. Materials and Methods

Amorphous Fe73.9Cu1Nb3Si15.5B6.6 and Fe81.2Co4Si0.5B9.5P4Cu0.8 ribbons (called thereafter alloy A, and alloy B, respectively) fabricated by single-roller melt spinning were supplied by Vacuumschmelze GmbH, Hanau, Germany.
First, thermomechanical analyses were performed on the amorphous tape material using differential scanning calorimetry (DSC) and dynamic mechanical analysis (DMA). The characteristic temperatures for the crystallization Tx,n as well as their respective activation enthalpies Ea,n were determined by DSC (Pegasus 404 F1, Netzsch, Selb, Germany). For these investigations, heating rates of 5, 10, 20, and 50 K/min were used in a temperature range of 323–1273 K. The background correction of the DSC measurements was carried out by subtracting two consecutive heating cycles and using the second cycle as a baseline.
Second, dynamic mechanical analysis (DMA), applied by the Discovery Hybrid Rheometer DHR 3 (TA Instruments) in tension mode, was used to determine the glass transition temperature Tg, which is difficult to be exactly determined by DSC because, for most Fe-based amorphous alloys, for the change in heat capacity during the glass, the transition is small (e.g., [24]). The measurements were conducted for different frequencies in a range of 0.1–10 Hz in a temperature range of 313–873 K.
For the HPT experiments, a custom-made facility with 400 kN capacity, equipped with an induction heating system (e.g., [33,34]) was used (Figure 1). 22 µm thick ribbons were cut in squares of 12 × 12 mm2 from both alloys and stacked between two tungsten carbide HPT anvils with a flat top of 8 mm diameter.
The samples were deformed in torsion at the conditions according to Table 1. The deformation temperature, Tdef, the maximum number of turns, N, and the applicable pressure, p, were limited by the material properties of the tungsten carbide anvils.
Macro torsional shear strains, γtorsion, were calculated according to Equation (1) (see [34,35]):
γ t o r s i o n =   2 π N r t
The thickness of the HPT disc, t, from which the samples for the consecutive measurements were taken, was evaluated by light microscopy. The torsional shear strains and corresponding disc radii, r, as well as the number of HPT turns, N, are listed in Appendix A of this paper (see Table A1 for alloy A and Table A2 for alloy B).
X-ray diffraction (XRD) measurements were performed using a benchtop XRD system with Co Kα anode and Fe Kβ-filter (Bruker D2 Phaser, Karlsruhe, Germany). After the experiment, the background and Kα2 contribution were separated from the measured data. The crystallite size D was analyzed via the Scherrer Equation (2) where K is the shape factor, λ is the X-ray wavelength, β is the full width at the half maximum of the investigated peak and θ is the position of that peak (see e.g., [36] for more details).
D = K λ β cos θ
Cross-sections of the HPT-processed samples were mechanically polished for analysis by optical light microscopy (Olympus BX 51 M) and scanning electron microscopy (LEO 1525, Zeiss, Oberkochen, Germany) to investigate the homogeneity of deformation after HPT and possible crack formation. Investigation of ultrafine-grained/nanocrystalline microstructures required careful transmission electron microscopy (TEM) analyses. For this purpose, FIB lamellae were prepared using an FEI Helios NanoLab 660 dual-beam workstation. The microscope was run at voltages 30–2 kV and Ga+ currents ranging from 50 nA (coarse milling) to 50 pA (polishing). High-resolution TEM images, selected area diffraction patterns, and bright-field scanning TEM (STEM) micrographs were recorded using an FEI Themis TEM. The microscope was operated at an accelerating voltage of 300 kV and a probe current of 0.1 nA. Lamellae were cut 1 mm from the samples’ edges.

3. Results

3.1. Alloy A—Fe73.9Cu1Nb3Si15.5B6.6

In an earlier work [32] we investigated the effect of HPT deformation on the Fe73.9Cu1Nb3Si15.5B6.6 alloy. Because of the high strength of the ribbons [25], HPT deformation was limited to one turn, irrespective of pressure and temperature. In the present work, we present an optimized setup, using flat tungsten carbide anvils, which allows us to observe the microstructural changes up to much larger torsional shear strains.
After HPT deformation, the samples were checked for homogeneity by analyzing the cross-section by optical microscopy (Figure 2).
The elliptic shape of the HPT sample is a consequence of the flow pattern, when flat HPT anvils are used for the deformation procedure. However, as visible from the light microscope image even for the highest degree of deformation (e.g., N = 10 and γtorsion = ~3400), no large-scale cracking did occur, probably due to the fact that the tungsten carbide anvils allow us to provide a maximum HPT pressure of 4 GPa. Moreover, it seems that the increase of the HPT deformation temperature to 473 K (about 60% of the glass transition temperature) provides sufficient deformability, thus limiting the crack length to a few submicrons in size (compare [32]). 60% of the glass transition temperature corresponds to the region where metallic glasses typically show a transition from inhomogeneous to more homogeneous deformation [37].
At first, undeformed samples were investigated by XRD and compared to the deformed material after various HPT turns. The diffraction pattern of the undeformed state in Figure 3 does not change with an increasing number of HPT turns (N = 2, 5, 10), suggesting that no crystallization occurred. Thus, even though the samples have been HPT-deformed at 473 K (see Table 1) alloy A still remains amorphous.
Earlier DMA experiments on the undeformed state (as-spun Fe73.9Cu1Nb3Si15.5B6.6 ribbons) [32] revealed a glass transition temperature Tg of 740 ± 0.5 K [heating rate of 10 K/min] with the corresponding activation enthalpy Ea being 282 ± 28 kJ/mol.
The crystallization kinetics was further studied by DSC measurements in the temperature range from 323 K to 1273 K using a heating rate of 20 K/min. The DSC scans in Figure 4 compare HPT-deformed samples at N = 2, 5, 10 turns with the as-spun ribbon material. The two peak temperatures, Tx1 = 808 ± 5 K and Tx2 = 983 ± 5 K were found to have about the same activation enthalpy of 470 ± 20 kJ/mol (see [32]). According to literature (e.g., [13,21,38]) the first stage of crystallization corresponds to the precipitation of α-Fe and the intermetallic phase Fe3Si whereas the second one is related to the crystallization of the residual glass and the formation of Fe-borides. The temperatures of the peaks do not shift with a changing number of HPT turns, indicating that the microstructure beyond a certain degree of HPT deformation does not change anymore. This result agrees well with the XRD results (see Figure 3) where even the sample deformed at the highest number of turns (N = 10, γtorsion = ~3400) still shows an amorphous profile similar to that of the undeformed as-quenched state.
Further evidence for the amorphous state of alloy A after HPT deformation is provided by high-resolution TEM analyses. Figure 5a shows a high-resolution TEM image of a FIB lamella prepared from the highest deformation state (N = 10 corresponding γtorsion = ~3400). The uniform contrast therein clearly shows that no crystals formed at this deformation state. Further, the selected area diffraction pattern in Figure 5b appears blurred, indicating that the alloy stayed amorphous. In sum, the DSC measurements, as well as the XRD and TEM analyses confirm that alloy A exhibits no crystallization upon HPT deformation.

3.2. Alloy B—Fe81.2Co4Si0.5B9.5P4Cu0.8

Studying the phase evolution of Fe81.2Co4Si0.5B9.5P4Cu0.8 after the same number of HPT turns as imposed to alloy A but at 293 K reveals a completely different behavior. Figure 6 reveals that crystalline α-Fe ((110), (200), (211), (220)) develops with increasing HPT strain. The intensity of the crystalline peaks steadily increases after the first appearance after 2 HPT turns. These results suggest that with α-Fe only a single phase crystallizes. It is the desired soft magnetic phase; no peaks corresponding to the hard magnetic phases (e.g., borides) are visible. Furthermore, by means of the Scherrer Equation (2), a grain size of about 9 nm was calculated for the sample deformed to 10 turns, thus to the highest imposed strain.
The thermal characteristics of alloy B before HPT deformation were investigated by DSC and DMA. DSC was carried out by heating from room temperature to 1273 K at heating rates between 5 and 50 K/min, to evaluate the temperatures Tx,1 and Tx,2 at the peak positions of the first and second stage of crystallization, respectively. Both peak temperatures rise with increasing heating rate (Figure 7a) which—by means of Kissinger analysis [39]—allowed to determine the activation enthalpies as Ea1 = 240 ± 13 kJ/mol and Ea2 = 897 ± 263 kJ/mol.
An in-depth analysis of the glass transition behavior of the undeformed state of alloy B was conducted by DMA measurements, to the authors’ best knowledge for the first time. The storage modulus was measured at frequencies ranging from 0.1–10 Hz at a heating rate of 10 K/min (Figure 8a). The glass transition temperature Tg of alloy B (Fe81.2Co4Si0.5B9.5P4Cu0.8) was determined from the onset of the storage modulus drop (see arrows in Figure 8a). It rises with increasing frequency, yielding a glass transition temperature of Tg = 526 ± 0.5 K measured at 0.1 Hz. The corresponding activation enthalpy was determined as Ea,g = 151 ± 3 kJ/mol using the slope of the Arrhenius plot (Figure 8b). The strong linearity in the Arrhenius plot indicates that alloy B is a strong glass former in contrast to a fragile glass former that would show Vogel-Fulcher-Tammann-like behavior [40].
To study the crystallization behavior of the HPT-deformed samples of alloy B, DSC measurements were conducted after a different number of HPT turns (N = 1, 2, 5, and 10) and compared with the undeformed (as-quenched) state. HPT deformation was conducted at room temperature and under a pressure of 3 gPa according to Table 1.
In contrast to alloy A, alloy B shows a limited deformation behavior and higher brittleness, probably because of the deformation-induced crystallinity during HPT (compare remarks on hardness in Section 1, and refs. [5,25,26]). Light microscopy of the sample cross-sections revealed that the material is not crack-free (Figure 9). The crack in the center of the HPT disc spans over the entire sample cross-section and developed during the unloading of the HPT anvils.
The DSC curves in Figure 10 were collected at a heating rate of 20 K/min starting at room temperature up to 1273 K. With an increasing number of turns, the first peak shifts to lower temperatures, from 675 ± 5 K in the undeformed state to 668 ± 5 K after 5 turns, but the crystallization enthalpy decreases with increasing strain, entirely disappearing after 10 turns. This means that crystallization of the phase associated with that peak already occurs during HPT deformation, with a maximum of HPT-induced crystallization after 10 turns. The crystallization enthalpy of the second DSC peak does not change significantly with an increasing number of HPT turns, indicating that no HPT-induced crystallization of additional phases occurs.
For a direct structural analysis, STEM images were taken from a FIB lamella prepared from the highest deformation state achieved at (N = 10, γtorsion = ~2500). Figure 11a unambiguously shows that numerous crystals with a size of 6 (±1) nm develop in alloy B, covering about 50% of the whole sample volume. This crystal size matches the size estimated by the Scherrer equation (see Section 2). Figure 11b presents the corresponding selected-area diffraction pattern. There is an increased number of rings with slightly varying intensity, indicating nanocrystallization with minor orientation anisotropy.

4. Discussion

Summing up the results demonstrated in detail in the foregoing section clearly shows that the elastic and plastic deformation under elevated hydrostatic pressure—as it is usually provided by HPT—induces crystallization in alloy B (Fe81.2Co4Si0.5B9.5P4Cu0.8). Alloy A (Fe73.9Cu1Nb3Si15.5B6.6) under similar conditions, however, stays amorphous at comparable as well as very high shear strains. In what follows, the reason for this very different behavior of alloys A and B will be discussed.
First, we wish to emphasize that—for the example of alloy B—SPD driven crystallization has been convincingly demonstrated for the first time, by complementary evidence from differential scanning calorimetry, dynamic mechanical analysis, X-ray diffraction, and transmission electron microscopy. With the help of the latter results, one can even quantify the crystallization effect induced by HPT by estimating the volume fraction of crystalline phase as a function of applied HPT shear strain using the measured DSC and XRD data shown in Figure 7 and Figure 8, respectively.
The XRD measurements (Figure 6) of alloy B show that the undeformed state is completely amorphous. Kuhnt [5] reported that the maximum achievable crystalline volume fraction in alloy B does not exceed 55 vol.%. Therefore, we assumed a maximum crystallization of 55 vol.% for the sample after 10 HPT turns, because at this stage of HPT deformation the first DSC peak in Figure 7 corresponding to precipitation of the soft magnetic α-Fe phase (e.g., [13]) vanishes completely. By scaling the crystallization enthalpy—i.e., the area of this peak for N = 1, 2, 5, and 10 turns—with that of the undeformed state (100% amorphous = maximum area), the evolution of the crystallized volume fraction as a function of HPT deformation can be estimated, results of which are given in Figure 12.
Now, to understand the different effects of HPT on alloys A and B in question, let us consider the energy which is expended mechanically during HPT (Eexp) in each of both cases. For this purpose, in-situ HPT torque measurements of Vorhauer and Pippan [41] and Schniewind [42] can be used, which both show saturation of the torsional shear stress at least at the torsional shear strains achieved in this work. The latter can be determined from the sample thicknesses as well as the number of HPT turns, and then the Eexp values can be calculated from the fairly rectangular areas below the stress-strain curves (for details, see Appendix A). The resulting values of Eexp are shown as a function of strain for both alloys in Figure 13. There it can be seen that in alloy B (i) Eexp is larger at all torsional shear strains applied, and also that (ii) the alloy-specific activation Ea = 472 ± 10 kJ/mol is reached already at γtorsion = 36. These two facts may explain why in this alloy crystallization occurs easier than in alloy A where the values of expended energy at all torsional shear strains applied are smaller. This is not an effect of apparently different deformation temperatures which—in terms of their specific glass temperatures—are quite similar (alloy A: TH = 0.57, alloy B: TH = 0.64)—with TH here being the deformation Temperature Tdef given in units of the glass transition temperature Tg. More significantly seems to be that the activation enthalpy for crystallization in alloy A is almost twice as high—Ea = 472 ± 10 kJ/mol—than that of alloy B being Ea = 240 ± 13 kJ/mol. However, getting into detail with this explanation, two problems appear: (i) the crystallization in alloy B only appears beyond an HPT strain of γtorsion = ~580 and not already at γtorsion = 36, and (ii) deformation-induced crystallization should occur also in alloy A: the critical activation enthalpy of Ea = 472 ± 10 kJ/mol should be reached here at torsional strains of about γtorsion = ~90. However, even at the highest γtorsion = 3400 applied, crystallization did not occur (unless both the applied pressure and deformation temperature are significantly higher, for details see [32]). At this point we favor another explanation: Alloy A crystallizes in several phases, mainly in two ones, namely α-Fe and the intermetallic phase Fe3Si with large differences in the phase compositions requiring complex nucleation processes which cannot be assisted by plastic deformation alone, and hence represent a kinetic obstacle for the crystallization process. In contrast to that, in the case of alloy B, only one crystallization peak of the α-Fe phase is found (e.g., see [4,26]), which has a comparably small difference to the initial phase composition and which can be easily overcome by deformation energy in the kinetic window provided by the HPT process. This explanation is confirmed if we inspect the existing literature on SPD-induced nanocrystallization: Several melt-spun Al alloys [43,44] which show only one crystallization peak during heating, exhibit crystallization during/after HPT processing; the same is true for a CuZrTi glass [45]. In contrast to that, all the investigations on Vitroperm-type alloys show SPD-induced crystallization only at higher pressures (at least 6 gPa [46]) or higher pressures (7.5 gPa) and elevated temperatures equal to or larger than 300 °C (573 K) [32]. There seems to be only one exception represented by the work of Aronin et al. [14,29] who reported substantial deformation-induced nanocrystallization at RT in Fe78Si13B9 which however—in contrast to alloy A—does not contain Cu and Nb. This alloy crystallizes in two stages with activation energies of Ea ~325 ± 5 K for both [47]. Compared to alloy A, this indicates an easier start of the crystallization process, and compared to alloy B a harder start of the crystallization process.
Finally, it should be emphasized that these features should allow for significant improvements in the magnetic properties of Fe-based glasses, at least of the ‘Makino’-type-alloy Fe81.2Co4Si0.5B9.5P4Cu0.8. Related results will be reported in a forthcoming paper [48].

5. Summary and Conclusions

Concerning energy efficiency for transformer and sensor applications, iron-based metallic glasses are among the best soft magnetic materials because of their low coercivity. However, saturation polarization is known to be limited. Former strategies to specifically heat the material for partial nanocrystallization were successful; however, the whole preparation process appears extensive and rather complicated for commercial production. Therefore, this paper considered the potential of SPD to trigger crystallization, thus simplifying the processing scheme. For this purpose, this paper investigated the microstructural response of two important glassy alloys, A (Fe73.9Cu1Nb3Si15.5B6.6 “Vitroperm”) and B (Fe81.2Co4Si0.5B9.5P4Cu0.8 “Makino”). Efforts at first focused on the realization of bulk glassy samples by HPT, by consolidation from amorphous melt-spun ribbons and/or quenched foils. In a previous paper, we have shown that applying HPT to alloy A (Fe73.9Cu1Nb3Si15.5B6) fulfills this goal. With this paper, we showed that the thickness of the sample can be even further increased by extension of the HPT parameters and that also other glassy alloys (alloy B, “Makino”) can be turned into massive shapes. Further results are as follows:
  • For alloy B (“Makino” Fe81.2Co4Si0.5B9.5P4Cu0.8) it is even possible to partially crystallize it as α-Fe precipitates at room temperature by means of HPT, with an upper limit of about 50 vol.% crystallinity of crystals with about 6 nm size. This crystal size is significantly lower than that received so far by conventional annealing procedures; moreover, HPT opens better possibilities for precise tuning of crystallinity and crystal size, which seems important for the tuning of the magnetic properties as well.
  • For alloy A (“Vitroperm” Fe73.9Cu1Nb3Si15.5B6.6), HPT crystallization is not possible even at the highest HPT parameter values chosen, because of the quasi-simultaneous crystallization of two phases and compositional differences between crystalline and amorphous phases in case of alloy A (“Vitroperm”) compared to the case of alloy B (“Makino”) alloy. These large differences result in a kinetic barrier that cannot be overcome by HPT deformation.
As already mentioned, a forthcoming paper will report on the HPT-induced changes in magnetic properties [48].

Author Contributions

Conceptualization, M.A., C.P., R.P., M.J.Z. and J.E.; methodology, M.A., F.S., P.R., R.P. and M.J.Z.; formal analysis, M.A., F.S., C.G., M.K. and N.P.; writing—original draft preparation, M.A. and F.S.; writing—review and editing M.A., F.S., M.J.Z. and J.E.; supervision, J.E., F.S. and M.J.Z.; funding acquisition, J.E. All authors have read and agreed to the published version of the manuscript.

Funding

We would like to thank the European Research Council, Grant ERC-2013-ADG-340025 for their support and cooperation. Funding from the Austrian Academy of Sciences via the Innovation Fund project IF 2019–37 is gratefully acknowledged. We acknowledge CzechNanoLab Research Infrastructure supported by MEYS CR (LM2018110). P.R. would like to acknowledge project no. 2020-4.1.1-TKP2020 supported by the Ministry of Innovation and Technology of Hungary via the National Research, Development, and Innovation Fund, financed under the TKP 2020 funding scheme.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

The raw data presented in this study will be made available on reasonable request to the corresponding author.

Acknowledgments

This paper is dedicated to the memory of Roland Grössinger who unfortunately passed away during the work for this paper. He made seminal contributions to the conceptualization and formulation of the methodology of this paper.

Conflicts of Interest

The authors declare no conflict of interest. The funders had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript, or in the decision to publish the results.

Appendix A

Estimations of the energy expended during the HPT process of the two alloys given in Figure 13 were undertaken based on in-situ HPT torque measurements of Vorhauer and Pippan [41] on ARMCO Fe and Schniewind [42] on 316 LVM alloyed steel. The latter was used for representing the strength at RT of both alloys A and B, and the measurements of Vorhauer and Pippan provided the dependence of torque on the HPT temperature. The expended deformation energy was estimated from the area under the torsional shear stress/strain curve being close to a rectangle. As the torsional shear stress depends linearly on the torque [49], its values could be estimated for both room temperature (RT) and higher temperatures—especially that of 453 K being close to the HPT temperature applied in the case of alloy A (473 K). The torsional shear strains were calculated by Equation (1) using the number of turns and the measured thicknesses given in Table A1 and Table A2, while those and the sample diameter as well as the specific densities of the alloys gave the masses necessary for the calculation of the expended energy Eexp.
Table A1. Expended energy Eexp estimated from torque measurements done during HPT, for alloy A.
Table A1. Expended energy Eexp estimated from torque measurements done during HPT, for alloy A.
Number of TurnsThickness [µm]Torsional Shear Stress [MPa]Torsional Shear Strain [1]Eexp
@ 453 K [kJ/mol]
1156673.4161844.2
287 5783027.7
570 17959407.4
1074 339617,797.7
Table A2. Expended energy Eexp estimated from torque measurements done during HPT, for alloy B.
Table A2. Expended energy Eexp estimated from torque measurements done during HPT, for alloy B.
Number of TurnsThickness [µm]Shear Stress [MPa]Shear StrainEexpend
@ RT [kJ/mol]
1238897.8106716.8
2146 3442337.1
5116 10837353.8
10100 251317,060.7

References

  1. Makino, A. Nanocrystalline soft magnetic Fe–Si–B–P–Cu alloys with high B of 1.8–1.9 T contributable to energy saving. IEEE Trans. Magn. 2012, 48, 1331–1335. [Google Scholar] [CrossRef]
  2. Yoshizawa, Y.; Oguma, S.; Yamauchi, K. New Fe-based soft magnetic alloys composed of ultrafine grain structure. J. Appl. Phys. 1988, 64, 6044–6046. [Google Scholar] [CrossRef]
  3. Groessinger, R.; Sato-Turtelli, R.; Duong, V.H.; Kuß, C.; Polak, C.; Herzer, G. Temperature dependence of the magnetostriction in α-Fe(100-x)Six and FINEMET type alloys. J. Metastab. Nanocryst. Mater. 1999, 1, 135–142. [Google Scholar] [CrossRef]
  4. Kuhnt, M.; Marsilius, M.; Strache, T.; Polak, C.; Herzer, G. Magnetostriction of nanocrystalline (Fe,Co)–Si–B–P–Cu alloys. Scr. Mater. 2017, 130, 46–48. [Google Scholar] [CrossRef]
  5. Kuhnt, M. Structural and Magnetic Characterization of Fe–Si–B–P–Cu Alloys. Ph.D. Thesis, Technische Universität, Darmstadt, Germany, 2019. [Google Scholar] [CrossRef]
  6. Flohrer, S.; Herzer, G. Random and uniform anisotropy in soft magnetic nanocrystalline alloys (invited). J. Magn. Magn. Mater. 2010, 322, 1511–1514. [Google Scholar] [CrossRef]
  7. Ayers, J.D.; Harris, V.G.; Sprague, J.A.; Elam, W.T.; Jones, H.N. On the formation of nanocrystals in the soft magnetic alloy Fe73.5Nb3Cu1Si13.5B9. Acta Mater. 1998, 46, 1861–1874. [Google Scholar] [CrossRef]
  8. Herzer, G.; Hilzinger, H.R. Surface crystallisation and magnetic properties in amorphous iron rich alloys. J. Magn. Magn. Mater. 1986, 62, 143–151. [Google Scholar] [CrossRef]
  9. Xue, Z.; Li, X.; Sohrabi, S.; Ren, Y.; Wang, W. Magnetic properties in Finemet-type soft magnetic toroidal cores annealed under radial stresses. Metals 2020, 10, 122. [Google Scholar] [CrossRef]
  10. Günther, W. Stress annealing process suitable for the production of low permeable nanocrystalline tape wound cores. J. Magn. Magn. Mater. 2005, 290–291, 1483–1486. [Google Scholar] [CrossRef]
  11. Herzer, G.; Flohrer, S.; Polak, C. Effect of stress annealing on the saturation magnetostriction of nanocrystalline Fe73.5Cu1Nb3Si15.5B7. IEEE Trans. Magn. 2010, 46, 341–344. [Google Scholar] [CrossRef]
  12. Herzer, G. Magnetic field-induced anisotropy in nanocrystalline Fe–Cu–Nb–Si–B alloys. J. Magn. Magn. Mater. 1994, 133, 248–250. [Google Scholar] [CrossRef]
  13. Gavrilović, A.; Minić, D.M.; Rafailović, L.D.; Angerer, P.; Wosik, J.; Maričić, A.; Minić, D.M. Phase transformations of Fe73.5Cu1Nb3Si15.5B7 amorphous alloy upon thermal treatment. J. Alloys Compd. 2010, 504, 462–467. [Google Scholar] [CrossRef]
  14. Abrosimova, G.; Aronin, A.; Matveev, D.; Pershina, E. Nanocrystal formation, structure and magnetic properties of Fe–Si–B amorphous alloy after deformation. Mater. Lett. 2013, 97, 15–17. [Google Scholar] [CrossRef]
  15. Zehetbauer, M.; Zhu, Y.T. Bulk Nanostructured Materials; Wiley-VCH Weinheim: Hoboken, NJ, USA, 2008; ISBN 978-3-527-31524-6. [Google Scholar]
  16. Edalati, K.; Bachmaier, A.; Beloshenko, V.A.; Beygelzimer, Y.; Blank, V.D.; Botta, W.J.; Bryła, K.; Čížek, J.; Divinski, S.; Enikeev, N.A.; et al. Nanomaterials by severe plastic deformation: Review of historical developments and recent advances. Mater. Res. Lett. 2022, 10, 163–256. [Google Scholar] [CrossRef]
  17. Meng, F.; Tsuchiya, K.; Ii, S.; Yokoyama, Y. Reversible transition of deformation mode by structural rejuvenation and relaxation in bulk metallic glass. Appl. Phys. Lett. 2012, 101, 121914. [Google Scholar] [CrossRef]
  18. Bridgman, P.W. Effects of high shearing stress combined with high hydrostatic pressure. Phys. Rev. 1935, 48, 825–847. [Google Scholar]
  19. Spieckermann, F.; Şopu, D.; Soprunyuk, V.; Kerber, M.B.; Bednarcik, J.; Schökel, A.; Rezvan, A.; Ketov, S.; Sarac, B.; Schafler, E.; et al. Structure-dynamics relationships in cryogenically deformed bulk metallic glass. Nat. Commun. 2022, 13, 127. [Google Scholar] [CrossRef]
  20. Hono, K.; Hiraga, K.; Wang, Q.; Inoue, A.; Sakurai, T. The microstructure evolution of a Fe73.5Si13.5B9Nb3Cu1 nanocrystalline soft magnetic material. Acta Metall. Mater. 1992, 40, 2137–2147. [Google Scholar] [CrossRef]
  21. Herzer, G. Chapter 3: Nanocrystalline soft magnetic alloys. In Handbook of Magnetic Materials; Elsevier: Amsterdam, The Netherlands, 1997. [Google Scholar] [CrossRef]
  22. Khakwani, S.; Antoni, M.; Rabensteiner, A.; Schafler, E.; Grössinger, R.; Zehetbauer, M. Bulk nanocrystalline soft magnetic Fe–Si–X alloys achieved through severe plastic deformation. Materials 2022. to be submitted. [Google Scholar]
  23. Makino, A.; Kubota, T.; Yubuta, K.; Inoue, A.; Urata, A.; Matsumoto, H.; Yoshida, S. Low core losses and magnetic properties of Fe85-86Si1-2B8P4Cu1 nanocrystalline alloys with high B for power applications. J. Appl. Phys. 2011, 109, 07A302. [Google Scholar] [CrossRef]
  24. Stoica, M.; Eckert, J.; Roth, S.; Zhang, Z.F.; Schultz, L.; Wang, W.H. Mechanical behavior of Fe65.5Cr4Mo4Ga4P12C5B5.5 bulk metallic glass. Intermetallics 2005, 13, 764–769. [Google Scholar] [CrossRef]
  25. Glezer, A.M.; Shurygina, N.A. Amorphous-Nanocrystalline Alloys; Taylor & Francis Group: Boca Raton, FL, USA, 2017. [Google Scholar] [CrossRef]
  26. Minnert, C.; Kuhnt, M.; Bruns, S.; Marshal, A.; Pradeep, K.G.; Marsilius, M.; Bruder, E.; Durst, K. Study on the embrittlement of flash annealed Fe85.2B9.5P4Cu0.8Si0.5 metallic glass ribbons. Materials 2017, 156, 252–256. [Google Scholar] [CrossRef]
  27. Kovac, J.; Petrovič, P.; Fechová, E.; Füzer, J.; Kollár, P. Magnetic properties of the FINEMET type powder prepared by long time milling. Phys. Stat. Solidi (a) 2002, 189, 859–863. [Google Scholar] [CrossRef]
  28. Csach, K.; Miškuf, J.; Juríková, A.; Janák, G. Influence of plastic deformation on nanocrystallization of Finemet alloy. Acta Phys. Pol. A 2010, 118, 820–822. [Google Scholar] [CrossRef]
  29. Pershina, E.A.; Abrosimova, G.E.; Aronin, A.S.; Matveev, D.V. Evolution of magnetic properties of amorphous Fe78Si13B9 alloy during deformation and subsequent heat treatment. Phys. Solid State 2015, 57, 234–238. [Google Scholar] [CrossRef]
  30. Aronin, A.; Abrosimova, G.; Matvev, D.; Rybchenko, O. Structure and properties of nanocrystalline alloys prepared by high pressure torsion. Rev. Adv. Mater. Sci. 2010, 25, 52–57. [Google Scholar]
  31. Abrosimova, G.E.; Aronin, A.S.; Dobatkin, S.V.; Zver’kova, I.I.; Matveev, D.V.; Rybchenko, O.G.; Tat’yanin, E.V. Nanocrystallization of an amorphous Fe80B20 alloy during severe plastic deformation. Phys. Solid State 2007, 49, 1034–1039. [Google Scholar] [CrossRef]
  32. Antoni, M.; Spieckermann, F.; Soprunyuk, V.; Chawake, N.; Sarac, B.; Zalesak, J.; Polak, C.; Gammer, C.; Pippan, R.; Zehetbauer, M.; et al. Effect of high pressure torsion on crystallization and magnetic properties of Fe73.9Cu1Nb3Si15.5B6.6. J. Magn. Magn. Mater. 2021, 525, 167679. [Google Scholar] [CrossRef]
  33. Scheriau, S.; Zhang, Z.; Kleber, S.; Pippan, R. Deformation mechanisms of a modified 316L austenitic steel subjected to high pressure torsion. Mater. Sci. Eng. A 2011, 528, 2776–2786. [Google Scholar] [CrossRef]
  34. Pippan, R.; Scheriau, S.; Hohenwarter, A.; Hafok, M. Advantages and limitations of HPT: A review. Mater. Sci. For. 2008, 584–586, 16–21. [Google Scholar] [CrossRef]
  35. Beygelzimer, Y.; Kulagin, R.; Toth, L.S.; Ivanisenko, Y. The self-similarity theory of high pressure torsion. Beilstein J. Nanotechnol. 2016, 7, 1267–1277. [Google Scholar] [CrossRef]
  36. Warren, B.E. X-ray Diffraction; Dover Publications: New York, NY, USA, 1990; ISBN 978-0-486-66317-3. [Google Scholar]
  37. Spaepen, F. A microscopic mechanism for steady state inhomogeneous flow in metallic glasses. Acta Metall. Mater. 1977, 25, 407–415. [Google Scholar] [CrossRef]
  38. Shivaee, H.A.; Hosseini, H.R.M. Advanced isoconversional kinetics of nanocrystallization in Fe73.5Si13.5B9Nb3Cu1 alloy. Thermochim. Acta 2009, 494, 80–85. [Google Scholar] [CrossRef]
  39. Kissinger, H.E. Reaction kinetics in differential thermal analysis. Anal. Chem. 1957, 29, 1702–1706. [Google Scholar] [CrossRef]
  40. Angell, C.A. Formation of glasses from liquids and biopolymers. Science 1995, 267, 1924–1935. [Google Scholar] [CrossRef]
  41. Vorhauer, A.; Pippan, R. On the onset of a steady state in body-centered cubic iron during severe plastic deformation at low homologous temperatures. Metall. Mater. Trans. A 2007, 39, 417–429. [Google Scholar] [CrossRef]
  42. Schniewind, J.D. Strain-Rate Sensitivity in High Pressure Torsion of Steel, Iron and Nickel. Ph.D. Thesis, University of Vienna, Vienna, Austria, 2021. [Google Scholar] [CrossRef]
  43. Boucharat, N.; Hebert, R.; Rösner, H.; Valiev, R.Z.; Wilde, G. Synthesis routes for controlling the microstructure in nanostructured Al88Y7Fe5 alloys. J. Alloys Compd. 2007, 434–435, 252–254. [Google Scholar] [CrossRef]
  44. Kovács, Z.; Henits, P.; Zhilyaev, A.P.; Révész, Á. Deformation induced primary crystallization in a thermally non-primary crystallizing amorphous Al85Ce8Ni5Co2 alloy. Scr. Mater. 2006, 54, 1733–1737. [Google Scholar] [CrossRef]
  45. Révész, Á.; Hóbor, S.; Szabó, P.J.; Zhilyaev, A.P.; Kovács, Z. Deformation induced crystallization in an amorphous Cu60Zr20Ti20 alloy by high pressure torsion. Mater. Sci. Eng. A 2007, 460–461, 459–463. [Google Scholar] [CrossRef]
  46. Chu, F.; Wu, K.; Meng, Y.; Edalati, K.; Lin, H.-J. Effect of high-pressure torsion on the hydrogen evolution performances of a melt-spun amorphous Fe73.5Si13.5B9Cu1Nb3 alloy. Int. J. Hydrogen Energy 2021, 46, 25029–25038. [Google Scholar] [CrossRef]
  47. Dos Santos, D.S.; dos Santos, D.R. Crystallization kinetics of Fe–B–Si metallic glasses. J. Non Cryst. Solids 2002, 304, 56–63. [Google Scholar] [CrossRef]
  48. Antoni, M.; Spieckermann, F.; Plutta, N.; Ramasamy, P.; Polak, C.; Kunca, B.; Skorvanek, I.; Pippan, R.; Zehetbauer, M.; Eckert, J. Influence of high pressure torsion on the magnetic properties of two Fe-based metallic glasses. Nanomaterials 2023. to be submitted. [Google Scholar]
  49. Stüwe, H.-P.; Turck, H. Zur Messung von Fliesskurven im Torsionsversuch. Int. J. Mater. Res. 1964, 55, 699–703. [Google Scholar] [CrossRef]
Figure 1. Working principle of HPT with flat top anvils, up to 50 ribbons were stacked between the anvils for HPT consolidation.
Figure 1. Working principle of HPT with flat top anvils, up to 50 ribbons were stacked between the anvils for HPT consolidation.
Materials 16 01260 g001
Figure 2. Cross-section of Fe73.9Cu1Nb3Si15.5B6.6 after HPT-deformation at 473 K and 10 turns.
Figure 2. Cross-section of Fe73.9Cu1Nb3Si15.5B6.6 after HPT-deformation at 473 K and 10 turns.
Materials 16 01260 g002
Figure 3. X-ray diffraction patterns of alloy A (Fe73.9Cu1Nb3Si15.5B6.6) before (as-quenched) and after HPT-deformation at N = 2, 5, and 10. The positions of the expected crystalline peaks for α-Fe are indicated to highlight that the sample remains amorphous.
Figure 3. X-ray diffraction patterns of alloy A (Fe73.9Cu1Nb3Si15.5B6.6) before (as-quenched) and after HPT-deformation at N = 2, 5, and 10. The positions of the expected crystalline peaks for α-Fe are indicated to highlight that the sample remains amorphous.
Materials 16 01260 g003
Figure 4. Constant-rate heating DSC scans (heating rate 20 K/min) of alloy A (Fe73.9Cu1Nb3Si15.5B6.6) before (as-quenched) and after HPT deformation at N = 2, 5, and 10.
Figure 4. Constant-rate heating DSC scans (heating rate 20 K/min) of alloy A (Fe73.9Cu1Nb3Si15.5B6.6) before (as-quenched) and after HPT deformation at N = 2, 5, and 10.
Materials 16 01260 g004
Figure 5. High-resolution TEM image of a FIB-lamellae (a) and the corresponding selected-area diffraction pattern (b) of alloy A (Fe73.9Cu1Nb3Si15.5B6.6) deformed by HPT at 473 K for 10 turns.
Figure 5. High-resolution TEM image of a FIB-lamellae (a) and the corresponding selected-area diffraction pattern (b) of alloy A (Fe73.9Cu1Nb3Si15.5B6.6) deformed by HPT at 473 K for 10 turns.
Materials 16 01260 g005
Figure 6. X-ray diffraction patterns of alloy B (Fe81.2Co4Si0.5B9.5P4Cu0.8) before and after HPT deformation (N = 1, 2, 5, and 10) at room temperature.
Figure 6. X-ray diffraction patterns of alloy B (Fe81.2Co4Si0.5B9.5P4Cu0.8) before and after HPT deformation (N = 1, 2, 5, and 10) at room temperature.
Materials 16 01260 g006
Figure 7. DSC measurements for alloy B (Fe81.2Co4Si0.5B9.5P4Cu0.8) before HPT deformation (a) DSC scans obtained at different heating rates (5, 10, 20, and 50 K/min) and (b) Kissinger plots for determination of the activation enthalpies E(ai) for both crystallization stages. Β denotes the heating rate in K/min and Tp the local minimum of the respective stage of crystallization for that heating rate.
Figure 7. DSC measurements for alloy B (Fe81.2Co4Si0.5B9.5P4Cu0.8) before HPT deformation (a) DSC scans obtained at different heating rates (5, 10, 20, and 50 K/min) and (b) Kissinger plots for determination of the activation enthalpies E(ai) for both crystallization stages. Β denotes the heating rate in K/min and Tp the local minimum of the respective stage of crystallization for that heating rate.
Materials 16 01260 g007
Figure 8. DMA measurements for Fe81.2Co4Si0.5B9.5P4Cu0.8 before HPT deformation (a) Storage modulus measured by DMA with varying frequency (0.1–10 Hz) at a heating rate of 10 K/min (only selected numeric values given due to visibility) (b) Arrhenius plot of the glass transitions from Figure 8a for the determination of the activation enthalpy of the glass transition.
Figure 8. DMA measurements for Fe81.2Co4Si0.5B9.5P4Cu0.8 before HPT deformation (a) Storage modulus measured by DMA with varying frequency (0.1–10 Hz) at a heating rate of 10 K/min (only selected numeric values given due to visibility) (b) Arrhenius plot of the glass transitions from Figure 8a for the determination of the activation enthalpy of the glass transition.
Materials 16 01260 g008
Figure 9. Cross-section of alloy B (Fe81.2Co4Si0.5B9.5P4Cu0.8) after HPT deformation at room temperature to N = 10.
Figure 9. Cross-section of alloy B (Fe81.2Co4Si0.5B9.5P4Cu0.8) after HPT deformation at room temperature to N = 10.
Materials 16 01260 g009
Figure 10. Constant-rate heating DSC scans (heating rate 20 K/min) of alloy B (Fe81.2Co4Si0.5B9.5P4Cu0.8) before (as-quenched) and after HPT deformation at N = 1, 2, 5, and 10.
Figure 10. Constant-rate heating DSC scans (heating rate 20 K/min) of alloy B (Fe81.2Co4Si0.5B9.5P4Cu0.8) before (as-quenched) and after HPT deformation at N = 1, 2, 5, and 10.
Materials 16 01260 g010
Figure 11. Bright-field STEM micrograph (a) and selected-area diffraction pattern (b) of alloy B (Fe81.2Co4Si0.5B9.5P4Cu0.8) after deformation at room temperature, at a pressure of 3 GPa, for 10 turns at a rotation speed of 0.1 turns/min.
Figure 11. Bright-field STEM micrograph (a) and selected-area diffraction pattern (b) of alloy B (Fe81.2Co4Si0.5B9.5P4Cu0.8) after deformation at room temperature, at a pressure of 3 GPa, for 10 turns at a rotation speed of 0.1 turns/min.
Materials 16 01260 g011
Figure 12. Evolution of the crystalline volume fraction in alloy B (Fe81.2Co4Si0.5B9.5P4Cu0.8) vs. the number of HPT turns calculated from the DSC data (for details, see text).
Figure 12. Evolution of the crystalline volume fraction in alloy B (Fe81.2Co4Si0.5B9.5P4Cu0.8) vs. the number of HPT turns calculated from the DSC data (for details, see text).
Materials 16 01260 g012
Figure 13. Expended energy Eexp for alloys A (black) and B (red), during HPT, plotted vs. the HPT strain γtorsion with the critical levels of respective activation enthalpies EA, for the first stage of crystallization indicated. For alloy B, crossing occurs at a significantly smaller HPT strain than for alloy A.
Figure 13. Expended energy Eexp for alloys A (black) and B (red), during HPT, plotted vs. the HPT strain γtorsion with the critical levels of respective activation enthalpies EA, for the first stage of crystallization indicated. For alloy B, crossing occurs at a significantly smaller HPT strain than for alloy A.
Materials 16 01260 g013
Table 1. HPT deformation parameters.
Table 1. HPT deformation parameters.
Fe73.9Cu1Nb3Si15.5B6.6
(Alloy A)
Fe81.2Co4Si0.5B9.5P4Cu0.8
(Alloy B)
Number of stacked ribbons5030
Deformation temperature200 °C (473 K)Room temperature (293 K)
Deformation speed0.2 turns/min0.1 turns/min
Deformation pressure4 GPa3 GPa
Number of turns1, 2, 5 and 10
Final thickness range70–156 µm100–238 µm
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Antoni, M.; Spieckermann, F.; Plutta, N.; Gammer, C.; Kapp, M.; Ramasamy, P.; Polak, C.; Pippan, R.; Zehetbauer, M.J.; Eckert, J. Can Severe Plastic Deformation Tune Nanocrystallization in Fe-Based Metallic Glasses? Materials 2023, 16, 1260. https://doi.org/10.3390/ma16031260

AMA Style

Antoni M, Spieckermann F, Plutta N, Gammer C, Kapp M, Ramasamy P, Polak C, Pippan R, Zehetbauer MJ, Eckert J. Can Severe Plastic Deformation Tune Nanocrystallization in Fe-Based Metallic Glasses? Materials. 2023; 16(3):1260. https://doi.org/10.3390/ma16031260

Chicago/Turabian Style

Antoni, Monika, Florian Spieckermann, Niklas Plutta, Christoph Gammer, Marlene Kapp, Parthiban Ramasamy, Christian Polak, Reinhard Pippan, Michael J. Zehetbauer, and Jürgen Eckert. 2023. "Can Severe Plastic Deformation Tune Nanocrystallization in Fe-Based Metallic Glasses?" Materials 16, no. 3: 1260. https://doi.org/10.3390/ma16031260

APA Style

Antoni, M., Spieckermann, F., Plutta, N., Gammer, C., Kapp, M., Ramasamy, P., Polak, C., Pippan, R., Zehetbauer, M. J., & Eckert, J. (2023). Can Severe Plastic Deformation Tune Nanocrystallization in Fe-Based Metallic Glasses? Materials, 16(3), 1260. https://doi.org/10.3390/ma16031260

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop