Next Article in Journal
Editorial Catalysts: Special Issue on Catalytic Pyrolysis
Next Article in Special Issue
Catalytic Applications of Clay Minerals and Hydrotalcites
Previous Article in Journal / Special Issue
Effect of Reduction Atmosphere on Structure and Catalytic Performance of PtIn/Mg(Al)O/ZnO for Propane Dehydrogenation
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Gas-Phase Hydrogenation of Furfural to Furfuryl Alcohol over Cu-ZnO-Al2O3 Catalysts Prepared from Layered Double Hydroxides

by
Guillermo R. Bertolini
1,
Carmen P. Jiménez-Gómez
2,*,
Juan Antonio Cecilia
2,* and
Pedro Maireles-Torres
2
1
Centro de Investigación y Desarrollo en Ciencias Aplicadas Dr. J. Ronco CINDECA-CCT La Plata-CONICET-UNLP, Calle 47 Nº 257, La Plata 1900, Argentina
2
Departamento de Química Inorgánica, Universidad de Málaga, Cristalografía y Mineralogía (Unidad Asociada al ICP-CSIC), Facultad de Ciencias, Campus de Teatinos, 29071 Málaga, Spain
*
Authors to whom correspondence should be addressed.
Catalysts 2020, 10(5), 486; https://doi.org/10.3390/catal10050486
Submission received: 15 April 2020 / Revised: 26 April 2020 / Accepted: 27 April 2020 / Published: 29 April 2020
(This article belongs to the Special Issue Catalytic Applications of Clay Minerals and Hydrotalcites)

Abstract

:
Several layered double hydroxides (LDHs) with general chemical composition (Cu,Zn)1−xAlx(OH)2(CO3)x/2·mH2O have been synthesized by the co-precipitation method, maintaining a (M2+/M3+) molar ratio of 3, and varying the Cu2+/Zn2+ molar ratio between 0.2 and 6.0. After calcination and reduction steps, Cu/ZnO/Al2O3 catalysts were synthesized. These catalysts were characterized by X-ray diffraction (XRD), transmission electron microscopy (TEM), H2 thermoprogrammed reduction (H2-TPR), N2 adsorption-desorption at −196 °C, N2O titration, X-ray photoelectron miscroscopy (XPS), NH3-thermoprogramed desorption (NH3-TPD) and CO2- thermoprogrammed desorption (CO2-TPD). The characterization data revealed that these catalysts are mainly meso-and macroporous, where Cu, ZnO and Al2O3 are well dispersed. The catalytic results show that these catalysts are active in the gas-phase hydrogenation of furfural, being highly selective to furfuryl alcohol (FOL) and reaching the highest FOL yield for the catalyst with a Cu2+/Zn2+ molar ratio of 1. In an additional study, the influence of the aging time on the synthesis of the LDHs was also evaluated. The catalytic data revealed that the use of shorter aging time in the formation of the LDH has a beneficial effect on the catalytic behavior, since more disordered structures with a higher amount of available Cu sites is obtained, leading to a higher yield towards FOL (71% after 5 h of time-on-stream at 210 °C).

1. Introduction

Layered double hydroxides (LDHs), also known as anionic-clays or hydrotalcites, are a group of inorganic lamellar compounds of basic nature. In the last decades, much attention is being paid to the study of these inorganic materials due to their chemical and structural properties, which make them useful in interesting applications, such as adsorbents, catalysts, anion exchangers or flame retardants, among others [1,2,3]. These materials exhibit high chemical stability, good biocompatibility and pH-dependent solubility [4]. The first LDH reported in the literature, discovered in 1842, was the mineral hydrotalcite [Mg6Al2(OH)16]CO3·4 H2O. This inorganic structure results from stacked brucite layers, Mg(OH)2, where some Mg2+ ions can be replaced by Al3+ ions, thus generating an excess of positive charge in layers, which must be counterbalanced by the presence of anions, mainly carbonates (CO32−), in the interlayer spacing [1,2,3].
The general formula of LDH is [M(II)1−xM(III)x(OH)2]x + [An − x/n]x−·mH2O, where M(II) are divalent cations (Mg2+, Zn2+, Cu2+, Ni2+) and M(III) are trivalent cations (Al3+, Fe3+, Cr3+). An− is an anion of charge n, and m is the stoichiometric value of co-intercalated water [1].
LDHs can be synthesized through several synthesis methods, such as co-precipitation, sol-gel, hydrothermal or urea hydrolysis, although the most usual method is co-precipitation, which can be performed at variable or constant pH [3].
Focusing only on the catalytic properties of LDHs themselves, these inorganic compounds can display both acid and basic sites [5,6]. However, the amount and strength of these acid/basic sites can be modified by thermal treatment, where dehydroxylation and decarbonation processes cause the collapse of the layered structure, leading to the formation of their respective metal oxides [6]. In addition, if any of M(II) or M(III) cations is easily reducible, it is feasible to obtain catalysts with metallic, acid and basic sites, in such a way that they can find a large spectrum of catalytic applications.
Among the great variety of catalytic processes that have emerged in the last century, the biomass valorization to produce high value-added chemicals is attracting the interest of many research groups, as a sustainable alternative to the use of fossil-based raw materials. This great interest has been prompted by the depletion of fossil fuels, which has led to the search and development of alternative sources that can satisfy both chemical and energy demands [7,8]. Biomass is the only feedstock that can replace fossil fuels, but many efforts are still required for the implementation and integration of these processes in the forthcoming biorefineries. However, the selection of a biomass source must be carried out with care and responsibility, since this biomass could interfere with the food chain, causing serious speculation problems and social imbalances. Taking into account these premises, lignocellulosic biomass, coming from agricultural waste, has emerged as an abundant, sustainable and non-edible source of energy, biofuels and chemicals [9]. Lignocellulose is composed by cellulose (40–50%), hemicellulose (20–35%) and lignin (15–25%), which can be extracted selectively by using several thermal, physical and chemical treatments [10].
Focusing only on the hemicellulose fraction, this can be isolated under mild hydrolysis treatment, leading, after depolymerization and hydrolysis, to the respective monosaccharides, mainly xylose [11,12]. Xylose, in turn, can also be dehydrated through homogeneous and/or heterogeneous catalysts to obtain furfural (FUR) as the main product [12,13]. After bioethanol, furfural is the second most produced compound in the sugar platform. The great interest in this organic compound lies in its chemical structure (an aldehyde group and a furan ring with α,β-unsaturations), which confer it a high reactivity [12]. Thus, furfural can be used as feedstock to give rise to a wide range of products with applications in fields, such as polymers, pharmacy, cosmetics, among others, through hydrogenation, oxidation, dehydration, decarbonylation or condensation reactions [12,14,15]. Thus, for instance, different environmentally friendly processes have been reported aimed at the furfural derivatization for the synthesis of valuable chemicals in aqueous media [16,17], as well as in in eco-sustainable removable media as deep eutectic solvents, by using homogeneous [18] or heterogeneous catalysts [19,20].
Among the products that can be derived from FUR, furfuryl alcohol (FOL) is the most important. It has been estimated that about 62% of FUR production is employed for the synthesis of FOL due to its importance in resin manufacture for the foundry industry and for chemicals [15]. Industrially, FOL has been synthesized through furfural hydrogenation using a copper chromite catalyst [21,22,23,24]. Another product obtained in high proportions during FUR hydrogenation is 2-methylfuran (MF) [12], which is also considered a valuable product as a biofuel additive and for the synthesis of heterocycles [15].
Despite the good performance of the commercial copper chromite catalyst, in the last decade, environmental awareness has led to the search for chromium-free catalysts, which can be more sustainable. As alternative, transition metal-based catalysts, e.g., Cu [25,26,27,28,29,30,31,32,33,34,35], Ni [28,35,36,37,38,39,40,41] or Pd [28,42,43] have been proposed to replace copper chromite. Generally, these metals have been dispersed on different supports. Both the hydrogenating character of the metal and the acid/base/redox properties of the support play a determining role in the activity and the product pattern, mainly for those processes where FUR hydrogenation takes place in the gas phase.
In this context, the design of LDHs as catalyst precursors, where some of their cations can be easily reducible, is a suitable approach for the development of active catalysts for FUR hydrogenation to obtain high value-added chemicals. Several authors have reported the synthesis of Ni-based hydrotalcites as efficient catalysts for this reaction, although the high hydrogenating nature of Ni sites [28] leads to a wide range of products, including a high proportion of carbonaceous deposits in many cases [35,36]. A suitable alternative could be the use of Cu-based hydrotalcites, since Cu active centers display a lower hydrogenating capacity, in such a way that the selectivity pattern can be easily controlled. In this sense, previous research has evaluated the role of Al source in the synthesis of Cu/ZnO/Al2O3 from their respective hydroxides, after calcination and reduction [44]. These authors achieved well dispersed Cu centers, which were selective towards FOL [44]. In the present work, a series of [CuZn1−xAlx(OH)2]x + [An − x/n]x−·mH2O hydrotalcites have been synthesized by coprecipitation method, with different Cu/Zn molar ratio, although the M(II)/M(III) molar ratio (M(II) is Cu(II) + Zn(II)) was 3 in all cases, since this value favors the formation of ordered LDH structures [1,2,3]. Moreover, the effect of other parameters, like aging time, was also evaluated for the synthesis of LDHs. Precursors were calcined and reduced, and then characterized and tested in the FUR hydrogenation, with special emphasis on the correlation between the amount of available metal sites and their catalytic behavior.

2. Characterization of the Catalysts

The identification of crystalline phases was carried out by powder X-ray diffraction. In all cases, the XRD patterns of LHDs synthesized (Figure 1) are similar to those reported in the literature [1,45]. The most intense peaks correspond to the typical basal (00l) planes, thereby, those located at 2θ (°) ≈ 12, 24 and 34 are attributed to the (003), (006) and (009) planes. These can be indexed in a rhombohedral symmetry, which is assigned to a (Cu,Zn)1−xAlx(OH)2 (CO3)x/2 m H2O layered double hydroxide (Powder Diffraction File: PDF: 00-37-0629). In addition, less intense peaks ascribed to non-basal planes of hydrotalcites are also observed, together with other low intense peaks, mainly in those LDHs whose Cu2+ or Zn2+ content is higher. Thus, in the case of Cu-rich LDH, diffraction peaks attributed to copper(II) hydroxide are presented, while Zn-rich LDH also exhibits broad and poorly defined diffraction peaks attributed to zinc hydroxycarbonate.
CuZnAl-based hydrotalcites have been previously studied by FTIR and Raman spectroscopies, demonstrating that the Cu/Zn molar ratio influences their microstructure. Thus, higher Cu/Zn ratios lead to more homogeneous CuZnAl hydrotalcites, while lower values give rise to less homogeneous structures due to its composition is closer to pure ZnAl and CuAl hydrotalcites [46]. This latter could provoke the asymmetric broadening of Bragg peak profiles of LDH for lower Cu/Zn molar ratio, also characteristic of the stacking disorder for Zn-rich compounds (Figure 1). Moreover, this Raman study also confirmed the presence of carbonate species, not only as counterion in the interlayer region of LDH, but also in partial segregated malachite for high Cu/Zn molar ratios, which is in agreement with XRD data [46]. Following the procedure described by Santos et al. for (Cu,Zn)1−xAlx(OH)2(CO3)x/2·mH2O LDHs [46], these layered materials were thermally treated at 300 °C for 4 h. In their XRD patterns (Figure 2), a broadening of the diffraction peak in comparison to their respective LDHs is noticeable, as a consequence of the stacking disorder of the layered structure due to decarbonation and dehydroxylation of the LDH, leading to the typical diffraction peaks of their mixed metal oxides [1]. Thus, XRD profiles reveal an evolution from the calcined Cu-rich (P-CuZn_6) to the Zn-rich (P-CuZn_0.2) sample. In this sense, the XRD pattern of calcined P-CuZn_6 displays defined bands located at 2θ (°) = 32.5, 35.5, 38.7, 48.8, 53.5, 58.3, 61.6, 66.2 and 68.1 assigned to CuO (PDF: 00-048-1548). The progressive increase in Zn content gives rise to a much more amorphous XRD pattern, being only a broad band observed at 2θ (°) ≈ 33. These data suggest that calcined P-CuZn_2.5, P-CuZn_1 and P-CuZn_0.4 display a more amorphous structure, or are formed by smaller particles than that the calcined P-CuZn_6. For the calcined LDH with the highest Zn content (P-CuZn_0.2), broad bands at 2θ (°) = 31.8, 34.4, 36.2, 48.3, 56.5, 63.1 and 68.2, start to emerge. These peaks are assigned to hexagonal ZnO (PDF: 00-36-1451). On the other hand, no diffraction peaks could be ascribed to the presence of crystalline Al species, in such a way that these species must be amorphous, or dispersed in the other phases.
Once the catalyst precursors were synthesized after subsequently calcined, H2-TPR analysis was carried out to determine the appropriate reduction temperature to obtain the Cu0-based catalysts (Figure 3). It has been previously reported that usually it is not possible to discern the different stages of Cu reduction (Cu2+ → Cu+ → Cu0), so the different contributions observed are ascribed to Cu particles with different size and/or with different interaction with the support (ZnO/Al2O3) [26,30,34]. From the H2-TPR profiles, it can be inferred that the sample with the highest Cu content (CuZn_6) is more easily reducible than the rest of catalysts. Its reduction curve shows two well-defined reduction steps located at 185 and 240 °C, which can be explained by the co-existence of CuO particles with different interaction with the support, or particles with different size. As the Cu content decreases and the Zn content concomitantly increases, the H2-TPR profile progressively changes. Thus, it seems clear that the hydrogen consumption at low temperature progressively decreased, as observed for CuZn_2.5 and CuZn_1. In the case of CuZn_0.4, this low temperature band disappears, being only noticeable the presence of a single band whose maximum is located about 245 °C. Those catalysts with a lower proportion of Zn seem to be more reducible than the richer ones, thus indicating that the presence of ZnO would modify the electronic environment around CuO particles, as previously pointed out by other authors [47,48]. Previous research has reported that the reduction of Cu species in CuO/ZnO takes place about 210 °C [30], so Al species could exert an additional electronic promoter effect on the interaction between ZnO and CuO particles, in such a way that the reduction of Cu2+ species occurs at higher temperature, as was indicated in the literature [49]. On the other hand, as the catalyst with a lower Zn content is easily reducible, it is expected that Al species possess a less pronounced promoter effect than ZnO.
H2 consumption data of calcined P-CuZn_X materials are always lower than theoretical values, so a fraction of Cu2+ species could not be reduced (Table 1). In this sense, several authors have reported that the reduction of segregated metal carbonates can take place at high temperature, about 550 °C [46]. However, other authors have noted that Cu2+ ions could also be embedded in the octahedral sites of Al2O3, ZnO, or even ZnAl2O4, whose reduction should require a higher temperature [50,51].
Taking into account the H2-TPR profiles, the precursors were reduced at 300 °C, maintaining this temperature for 1 h to ensure the complete reduction of Cu2+ species.
XRD profiles of the CuZn_X catalysts show the typical diffraction peaks of the metallic Cu0 at 2θ (°) = 43.3 and 50.4 (PDF: 00-85-1326) (Figure 4). The presence of Cu2O should be discarded since, despite the main peak at 2θ (°) = 38.3 overlaps with a diffraction peak of ZnO, the secondary peaks of Cu2O do not appear, so partially reduced copper oxide (Cu2O) crystallites are not detected, or these are too small to be detected by XRD.
These signals are more defined than those corresponding to the hexagonal ZnO, which does not evolve to reduced Zn species. In the case of Al species, diffractograms do not reveal any characteristic peaks, so these Al species must be highly dispersed in the catalysts. The determination of the crystallite size for Cu0 was carried out from the Williamson-Hall equation [52], using the main diffraction peak at 2θ (°) = 43.3. The analysis of this (111) crystallographic plane reveals that the crystallinity of the Cu0 particles increases directly with the Cu content, from 5.0 nm for the lowest content (CuZn_0.2) to 28.8 nm for the highest (CuZn_6). These value are slightly lower than those observed for Cu/ZnO or Cu/MgO synthesized by the co-precipitation method [26,30], so Al species, in addition of exerting an electronic promoter effect, seem to favor the dispersion of Cu nanoparticles [49,53].
In order to elucidate the catalyst morphology, CuZn_X catalysts were analyzed by TEM (Figure 5). In all cases, the micrographs allow to distinguish different morphologies, including layered structures probably due to the hydrotalcite structure that did not fully collapse after the thermal treatment. These data are in agreement with the literature, where a proportion of the layered structure was reported to be maintained after the thermal treatment [54]. In addition, it is noticeable the presence of pseudospherical and well-dispersed nanoparticles, mainly in the samples with a higher Cu content. In both cases, these particles are very small, below 15 nm.
The analysis of these samples was also performed by Energy Dispersive X-Ray (EDX) (Figure 6). The images show that all elements (Cu, Zn, Al and O) are well dispersed in both lamellar and pseudospherical structures. In Figure 5 and Figure 6, it can be seen the existence of interparticle voids between adjacent nanoparticles.
The textural properties of CuZn_X catalysts were evaluated from their N2 adsorption-desorption isotherms at −196 °C (Figure 7A). According to the International Union of Pure and Applied Chemistry (IUPAC) classification [55], these isotherms can be considered as Type II, which are typical of macroporous solids, as suggests the great growing of N2 adsorbed at high relative pressure. The shape is similar for all CuZn_X catalysts, and, consequently, the modification of the Cu/Zn molar ratio does not seem to affect the textural properties of catalysts (Table 2). Thus, SBET values hardly vary, being between 70 and 85 m2 g−1, while t-plot data indicate that the surface ascribed to the microporosity can be considered as negligible, since values are below 10 m2 g−1 in all cases. In the same way, the pore volume is very similar for all catalysts, being in the range 0.474–0.679 cm3 g−1, while the micropore volume is very low in comparison to the total volume.
With regard to the pore size distribution, estimated by Density Functional Theory (DFT) [56] (Figure 7B), all CuZn_X catalysts follow the same pattern. The microporosity is barely appreciated, and only a small contribution appears at 1.2 nm. However, these samples exhibit a wide pore size distribution, extending from 3 to 150 nm, in such a way that these catalysts can be labeled as meso- and mainly macroporous. This porosity is ascribed to the voids between adjacent particles, as was suggested previously from the TEM micrographs (Figure 5 and Figure 6).
The quantification of surface Cu0 species of CuZn_X catalysts was carried out by N2O titration at 60 °C [57] (Table 3). The data indicate that dispersion decreases with the Cu content, going from 21% for CuZn_0.2 to 7% for CuZn_6. In the same way, the metallic surface area (m2Cu gCu−1) follows a similar trend, and the catalyst with the lowest Cu content (CuZn_0.2) displays the highest value. This study also reveals that the metal particle size increases directly with the Cu loading, from 5 nm for CuZn_0.2 to 19 nm for CuZn_6, being these data slightly lower than those obtained from XRD by using the Williamson-Hall method [52].
In order to determine the surface chemical composition of catalysts, X-ray photoelectron spectroscopy (XPS) analysis was carried out. Cu 2p core level spectra (Figure 8A) show that Cu 2p3/2 consists of a single contribution located at 932.0 eV, ascribed to reduced Cu species [30,32], since the absence of the typical shake-up satellite of divalent metals about 942–943 eV would exclude the existence of Cu(II) [58].
However, from this contribution, it is not possible to discern between Cu+ and Cu0 species, so the Auger CuLMM signal is used to identify these oxidation states [30,32]. The broad Auger CuLMM band (Figure 8B) can be deconvoluted in two main contributions: 918.5 eV, which is ascribed to Cu0, and 917.0 eV due to Cu+ [30]. The proportion of Cu0 increases directly with the Cu content, being about 65–70% of the total reduced Cu species. The analysis of the Zn 2p region (Table 4) evidences a single band between 1021.6–1022.1 eV, which is assigned to ZnO. Some studies of Cu/ZnO catalysts have demonstrated that ZnO can be partially reduced, arising a new contribution located at lower binding energy. This new band is not observed in the Zn 2p core level spectra; however, the Auger ZnLMM line (Figure 8C) shows an asymmetric band that would confirm the existence of a small proportion of Zn partially reduced (Znδ+), or even a synergistic effect between Cu0 and ZnO [59,60]. With regard to the Al 2p core level spectra, all CuZn_X catalysts display a contribution about 74.3 eV, which can be attributed to Al2O3 [61]. In the case of O 1s, all catalysts display a main contribution located about 531.0 eV, assigned to oxide species, and another less intense at 532.6 eV, that is assigned to hydroxyl and/or carbonate [61]. The existence of carbonates could be confirmed by the signal at a binding energy of 288–289 eV in the C 1s core level spectra [61], which could result from a low proportion of LDH, or a possible carbonation of the catalyst surface.
The atomic concentration data show that the surface Cu content progressive increases with the Cu loading, as expected (Table 4), although surface molar ratios seem to be lower than the theoretical values. This fact could be ascribed to both ZnO and Al2O3 exhibit a smaller crystallite size than Cu0, in such a way that both metal oxides should be better dispersed in catalysts. This fact can lead to lower than expected surface Cu concentrations.
As both acid and basic sites could also influence on the gas-phase FUR hydrogenation reaction, NH3-TPD and CO2-TPD studies were performed (Table 2). The NH3-TPD data show a relatively low amount of acid sites, decreasing from 78 μmol g−1 for CuZn_0.2 to 60 μmol g−1 for CuZn_6. The presence of these acid sites is ascribed to Al2O3 and Cu+, which provide Lewis acid sites, and even to ZnO due to its amphoteric character, similar to alumina. Several authors have reported that the modulation of the acidity plays a key role in FUR conversion, since a high number of acid sites can cause the polymerization of FUR, mainly in gas-phase, leading to the formation of a high proportion of carbonaceous deposits [29,37,62]. These polymerized FUR species interact strongly with the active sites, in such a way that catalysts tend to be deactivated relatively fast. However, the presence of weak acid sites could exert a beneficial effect on the catalytic behavior, since the interaction between FUR, or reaction products, and the catalyst is weakened in comparison with catalyst with higher acidity, thus favoring the desorption of products adsorbed on the catalyst surface. In this sense, several supports, such as SiO2 or clay minerals, with similar amount of acid sites [29,37], have provided good catalytic activity in FUR hydrogenation, under similar experimental conditions.
Similarly, a basic support (MgO, CaO, ZnO or CeO2) [25,26,30,63,64] also seems to have a positive effect in this catalytic process. CuZn_X catalysts display a small concentration of basic sites, between 15 and 39 μmol g−1, raising as the Cu content decreases. The presence of these basic sites is ascribed to the amphoteric character of both ZnO and Al2O3, as previously mentioned [65,66].

3. Catalytic Results

CuZn_X catalysts were tested in the gas-phase FUR hydrogenation, using FUR dissolved in cyclopentyl methyl ether (CPME). This solvent was selected due to its interesting physico-chemical properties, such as low solubility in H2O in comparison to other ethereal solvents, low formation of peroxides, low boiling point (106 °C) or relative high stability under acid or basic conditions [67]. Considering these premises, the first study was to evaluate the stability of the solvent under similar experimental conditions to those used for the catalytic evaluation of CuZn_X catalysts. At a reaction temperature of 190 °C, CPME was recovered without any modification, such as the cleavage of the –C–O–C– bond or isomerization.

3.1. Influence of Cu Content

Thereafter, CuZn_X catalysts were studied in the FUR hydrogenation at 190 °C (Figure 9). All the catalysts are prone to suffer a progressive deactivation, which could be a consequence of the strong interaction of FUR, or FOL molecules, with Cu active sites [68]. The catalyst with the lowest Cu content (CuZn_0.2) is also the least active catalyst, reaching a FUR conversion of 40% after 1 h of time-on-stream (TOS), which decreases until 26% after 5 h. By increasing the Cu content, the catalytic performance is clearly improved, since CuZn_0.4 attains a FUR conversion of 43% after 5 h of TOS, while CuZn_1 seems to be the most stable catalyst with a FUR conversion of 59%. However, this trend is not followed when the Cu content raises further, since both CuZn_2.5 and CuZn_6 catalysts exhibit a similar pattern, reaching a FUR conversion close to 50% after 5 h of TOS.
With regards to the selectivity pattern (Figure 9B,C), the modification of the Cu/Zn molar ratio hardly varies the ratio of the obtained products, since FOL always is the main compound, with a maximum yield of 55% for CuZn_1, after 5 h of TOS. In all cases, MF was also detected, although this can be considered a minority because MF yield did not exceed 6% after 5 h of TOS. The catalytic data can be compared with other catalysts reported in the literature. Thus, Cu/ZnO and Cu/CeO2 catalysts exhibited a high activity in the FUR hydrogenation, but the selectivity pattern is slightly different, since the amount of MF was higher in both cases [30,63]. Other authors have reported that the incorporation of Al2O3 exerts a promoter effect in the catalytic behavior due to Al species weaken the Cu-ZnO interaction [44]. This data could be in agreement with those obtained in the H2-TPR analysis, where the catalyst with a lower ZnO content (CuZn_6) is easily reducible. In earlier studies, Nagajara et al. established that co-precipitation is the most appropriate method to obtain a high dispersion of Cu species on a basic support like MgO [25]. These authors also reached a high activity in FUR conversion, with a high selectivity mainly towards FOL. In the same way, Dong et al. carried out a comparative study with Cu/ZnO, Cu/Al2O3 and Cu/SiO2 [29]. They concluded that the modification of the electronic density in the catalyst due to the Cu-support interaction has a determining role in the catalytic behavior, pointing out that the existence of weak acid sites favors MF formation, mainly in the case of Cu/SiO2, as a consequence of consecutive reactions (FUR → FOL → MF) [29]. These weak acid sites, associated to both the support and Cu+ sites, could be involved in the hydrogenolysis of FOL to MF due to their electron-deficiency [29,69]. Similar results were obtained by Jiménez-Gomez et al., who synthesized Cu/SiO2 catalyst by a complexation method to disperse Cu species [32]. They observed that, besides the presence of weak acid sites, it is necessary the existence of well-dispersed Cu nanoparticles, since the electron-deficiency of the catalyst enhanced [29,32]. In the present work, in spite of CuZn_X catalysts have acid sites, the amount of MF can be considered negligible in comparison to data reported in the literature [29,32]. In this sense, the catalysts highly selective towards MF display higher SBET values. This fact supposes a higher FUR-support interaction and consequently a longer residence time, which can favor consecutive reactions. CuZn_X catalysts showed lower SBET values and reduced porosity (Table 2 and Figure 7), mainly ascribed to their meso-macroporous nature. As the pore size is not modulated to the dimensions of the FUR molecule, the interaction FUR-active sites should be weaker, although this fact also has some advantage related to the presence of more labile sites that favor an easier desorption of FUR and products. This trend was also observed for other catalysts synthesized by co-precipitation method, such as Cu/MgO, Cu/ZnO or Cu/CeO2 [25,30,63]. The existence of Cu+ sites, as determined by XPS, does not favor the hydrogenolysis process to form MF, so it could be inferred that textural properties have a more determining role in the hydrogenolysis reaction than the amount of acid sites. However, the hydrogenation FUR → FOL takes place on the metallic sites [28,29] and it does not seem to be affected by the textural properties of catalysts. This fact was confirmed in Cu-based catalysts supported on clay minerals [33,37,70]. Thus, those catalysts with very poor textural properties, like bentonite, or whose pore dimensions hinder the incorporation of Cu nanoparticles, like sepiolite, only dispersed metal nanoparticles on the catalyst surface [33]. In both cases, the catalysts were selective towards FOL. However, the use of a clay mineral with less crystallinity as support led to higher SBET values due to an increase in the micro- and mesoporosity, thus favoring a higher interaction between FUR and the catalyst and longer residence time, in such a way that the reaction can evolve toward consecutive reaction steps [70]. In this sense, the formation of MF is favored by the existence of weak acid sites associated to the aluminosilicate, used as support, (kerolite) and the presence of a small fraction of Cu+ species. In these studies, the incorporation of promoters, such as ZnO, MgO or CeO2, modified the selectivity pattern, with an increase in the FOL yield due to milder interaction between support and Cu species, as indicated their H2-TPR data [29,37,70], which is in agreement with data reported in the present work.

3.2. Turnover Frequency (TOF)

In order to evaluate the activity of Cu sites, turnover frequency (TOF) data of catalysts were determined. It must be considered that most of catalysts are prone to suffer deactivation by the formation of carbonaceous deposits on the catalyst surface, and consequently the evaluation of the activity of these Cu sites only makes sense at zero time (t0), as long as these catalysts do not reach a total conversion at t0. In this sense, the linearization of the Figure 9A reveals that FUR conversion values vary between 43% for CuZn_0.2 and 76% for CuZn_2.5, at t0.
From the extrapolation to t0 (Figure 10A), it is feasible to determine the corresponding TOF values. The obtained data reveal that CuZn_0.2 displays the lowest TOF (28 h−1), whereas an increase in the Cu content improves TOF, and CuZn_0.4 and CuZn_1 show TOF values of 43 and 44 h−1 respectively. However, the use of larger Cu loadings worsens the efficiency of Cu active sites, since CuZn_2.5 and CuZn_6 reach TOF values of 36 and 37 h−1, respectively. In the same way, from the linearization of the data obtained in Figure 9A, it is possible to evaluate the amount of FUR converted per time unit and mass of catalyst at t0 (Figure 10B). These data reveal that the highest FUR rate was 1.113·10−2 mmol FUR g−1 h−1 for CuZn_1, while the poorest value was obtained for CuZn_0.2, with a rate of 0.678·10−2 mmol FUR g−1 h−1. In addition, from Figure 10B, an estimation of the catalyst lifetime can be made by extrapolation. These data reveal that the catalyst with longer life is CuZn_1, which could be active for 15.15 h. In this time, the catalyst could convert 0.1537 mmol FUR g−1 before exhaustion.

3.3. Influence of Reaction Temperature

Considering that CuZn_1 showed the longest lifetime, as well as the most efficient Cu active sites (Table 5), this catalyst was selected to evaluate the influence of the reaction temperature on the catalytic performance (Figure 11). FUR conversion clearly increases with the reaction temperature (Figure 11A), from 34% to 79% after raising the temperature from 170 to 230 °C, after 5 h of TOS. Several authors have reported that FUR hydrogenation is thermodynamically favored; however, the FUR conversion often displays a volcano shape with the reaction temperature, reaching a maximum conversion at 190–210 °C [27,62]. The worsening of the conversion at higher reaction temperature was attributed to FUR polymerization, due to its strong adsorption on the active sites involved in the hydrogenation process. This trend was not observed in the present work, which could be explained by the meso- and macroporosity of catalysts and the relatively low concentration of acid sites, in such a way that the FUR-active site interaction is weaker, so the desorption of FUR and reaction products should be easier [29,37,70]. With regard to the hydrogenation products (Figure 11B,C), in all cases, the main product was FOL, reaching a maximum yield of 65% after 5 h of TOS at 210 °C. MF yield values always were very low, although they increase slightly with the reaction temperature, attaining a maximum MF yield of 7% after 5 h of TOS at 230 °C [62]. Several authors have pointed out that the formation of MF is favored at higher reaction temperature (T > 190 °C) [25,30,62]. However, CuZn_1 hardly modifies its selectivity pattern when the reaction temperature increases, probably due to the weaker interaction between the active sites and FUR molecules. Thus, this catalyst seems to be highly stable and selective toward FOL, along the TOS, in a wide range of reaction temperatures [15].

3.4. Influence of Aging Time in the Synthesis

In the next study, the aging time of the LDHs was modified to evaluate its influence on the catalytic behavior. Thus, three CuZn_1 catalysts with different aging time (1, 48 and 168 h) were compared. The catalytic data show that longer aging time in the synthesis of LDHs has an adverse effect on the catalytic activity (Figure 12A). Thus, that LDH whose aging time was only 1 h gave rise to a catalyst that hardly undergoes deactivation, since it maintains a FUR conversion of 84% after 5 h of TOS at 210 °C. However, a more prolonged aging treatment (168 h) worsens the catalytic activity, achieving a FUR conversion of only 37%, under similar experimental conditions. The selectivity (Figure 12B,C) follows the same trend than that observed previously for CuZn_X catalysts, since FOL was the main product in all cases, attaining a maximum yield of 71%, after 5 h of TOS at 210 °C, with CuZn_1 aged for 1 h. The amount of MF was very low in all cases, although a decrease in MF yield took place as aging time was increased.
In order to understand the changes of the catalytic behavior for the CuZn_1 catalysts synthesized with different aging times, these catalysts were characterized. Their XRD patterns show clear differences in crystallinity (Figure 13A). Thus, the diffractogram of sample prepared with the shortest aging time (CuZn_1(1h)) does not display any diffraction peak, which are clearly visible for catalysts obtained by increasing the aging time. Thus, CuZn_1(168h) catalyst shows Cu crystallites of 33 nm. These data are in agreement with the literature, since the use of higher temperature and longer aging time favor the growing and better crystallization of layered double hydroxides [3,71]. This fact implies the formation of catalysts where nanoparticles of support and active phase are larger.
The analysis of the H2-TPR profiles also reveals clear modifications depending on the aging time (Figure 13B). Considering that the three catalysts display the same chemical composition, it is expected that the profile differences should be attributable to differences in the size of their Cu nanoparticles. In this sense, a catalyst whose Cu crystallite sizes are smaller (CuZn_1(1h)) is more easily reducible than those catalysts with bigger sizes, as a consequence of the weaker interaction between small CuO nanoparticles and the ZnO/Al2O3 support.
In addition, it is also noticeable that both CuZn_1(1h) and CuZn_1(48 h) catalysts display two defined peaks, which could point out the formation of Cu nanoparticles with two different sizes. However, CuZn_1(196h) only shows a peak at higher temperature. This fact could be ascribed to the use of longer aging time, which favors the formation of more homogenous structures. N2O titration data (Table 6) follow the trend observed by XRD and H2-TPR, since the catalyst with the lowest aging time (CuZn_1(1h)) is also the catalyst with a higher amount of available surface Cu sites. This would confirm the formation of smaller particles and consequently a higher metallic surface area is obtained, which is in agreement with its better catalytic performance.
Finally, the superficial analysis of these catalysts by XPS (Table 7) does not reveal any variation in core level spectra in comparison to CuZn_X catalysts. It is only noteworthy a decrease in the surface Cu content with the aging time, which can be explained by the formation of larger Cu nanoparticles, thus limiting the amount of Cu detected by XPS due to this technique only allows to analyze 2–3 nm of depth (Table 6). With regard to the oxidation state of Cu species, Cu0 is the main oxidation state, about a 70–75% of the total Cu, while the Cu+ is about 25–30%.

4. Materials and Methods

4.1. Preparation of Catalysts

A series of Cu/ZnO/Al2O3 catalysts has been synthesized by co-precipitation method, according to the methodology described by Santos et al. [46]. The LDH precursors were synthesized from aqueous solutions of Cu(NO3)2·2H2O (99%, Aldrich, Saint Louis, MI, USA), Zn(NO3)2·6H2O (99%, Aldrich) and Al(NO3)3·9H2O (99%, Aldrich) with a total metal concentration of 0.3 M. In all cases, (Cu2++Zn2+)/Al3+ molar ratio was 3, whereas the Cu2+/Zn2+ molar ratio was varied between 0.2 and 6. In the next step, an aqueous solution of Na2CO3 (1.0 M) was slowly added to precipitate metal hydroxides and form the LDH structure. Later, the obtained gel was aged at room temperature for 48 h (in two different synthesis, the gel was aged 1 and 168 h). The obtained solid was filtered and washed with distilled water until reach a neutral pH to ensure the total removal of Na+ ions. Finally, the solid was dried overnight at 90 °C and calcined at 300 °C for 4 h, using a ramp of 10 °C min−1.

4.2. Characterization of Catalysts

An X´Pert Pro automated diffractometer (PANanalytical, Bruker, Rheinstetten, Germany) was used to obtain powder X-ray diffraction patterns, this equipment are composed of a Ge (111) primary monochromator (Cu Kα1) and a X´Celerator detector with a step size of 0.017° (2θ), between 2θ = 10° and 70° with an equivalent counting time of 712 s per step. Williamson-Hall Equation (1) [52] was applied to calculate the crystallite size (D):
B cos θ = (Kλ/D) + (2 ε sin θ)
where B is the full width at half maximum (FWHM) of the XRD peaks, θ the Bragg angle, B is, K is the Scherrer constant, λ is the wavelength of the X ray and ε is the lattice strain.
A FEI Talos F200X (Thermo Fisher Scientific, Waltham, MA, USA) system was used to study the catalyst morphology by transmission electron microscopy (TEM). The images obtained with this technique show a high resolution; moreover, this equipment allows the combination of STEM and TEM imaging and, therefore, a 3D characterization with chemical composition mapping. The samples were dispersed in isopropyl alcohol and each one of them was put on a carbon grid.
The temperature of catalysts reduction was evaluated by H2-TPR (hydrogen temperature-programmed reduction). To carry out the experiments, 0.080 g of sample has been used. First, the catalyst precursor is treated under a He flow (35 mL min−1) at 100 °C for 30 min, after this, it is cooling to room temperature to start the analysis, where the H2 consumption is monitored between 50 and 800 °C, by using an Ar/H2 flow (48 mL min−1, 10 vol.% H2) with a heating rate of 10 °C min−1. An on-line thermal conductivity detector (TCD) (Shimadzu, Kioto, Japan) was used to carry out the H2 quantification. It is necessary to trap the water formed in the process to avoid equipment contamination, so the outcoming flow is passed through a cold finger immersed in a liquid N2/isopropanol bath (−80 °C).
In previous research [30,37], N2O titration has been employed to determine the metallic surface area and the dispersion of Cu0 species, where the superficial oxidation of Cu0 under a N2O flow takes place according to the Equation (2):
2Cu0 + N2O → Cu2O + N2
Prior to the analysis, the catalyst precursor was treated under a He flow (35 mL min−1) at 100 °C for 30 min, followed by a reduction step under a 10 vol.% H2/Ar-flow (48 mL min−1) at 300 °C for 1 h, with a heating rate of 5 °C min−1, being monitored the H2 consumption by TCD. When the catalyst was reduced, it was cooled until 60 °C under a He flow to carry out the Cu0 oxidation to Cu+ performed by titration N2O (5 vol.% N2O/He), at 60 °C for 1 h. At last, a second sample reduction was carried out by heating from room temperature to 300 °C with a heating rate of 5 °C min−1, being also monitored its H2 consumption by TCD.
The textural parameters were determined from the N2 adsorption-desorption isotherms at −196 °C by using an automatic ASAP 2020 Micromeritics apparatus (Micrometrics, Norcross, GA, USA). The sample was previously outgassed at 200 °C and 10−4 mbar for 12 h. The Brunauer-Emmet-Teller (BET) equation [72] was utilized to determine surface area taking a N2 cross section of 16.2 Å2. Micropore volume was determined from alpha-s- method. Pore size distribution was determined using the density functional theory (DFT) [56].
X-ray photoelectron spectra were obtained using a Physical Electronic PHI 5700 spectrometer (Physical Electronics, Eden Prairie, MN, USA), equipped with an Electronics 80-365B multichannel hemispherical electron analyzer and an Mg Kα X-ray excitation source (300 W, 15 kV, hv = 1253.6 eV). High-resolution spectra were recorded by a concentric hemispherical analyzer in a 29.35 eV constant energy mode, using a 720 µm diameter analysis area, and the pressure in the analysis chamber was kept below 5 × 10−6 Pa. Binding energies (BE) were determined to an accuracy of ± 0.1 eV, using the adventitious carbon C 1s signal at 284.8 eV as reference. PHI ACCESS ESCA-F V6 software (Eden Prairie, Minnesota, USA) was used for data acquisition and analysis. A Shirley-type background was subtracted from the signals. The recorded spectra were always analyzed with Gauss-Lorentz curves, in order to determine more precisely the binding energy of the atomic levels of the different elements. To avoid sample oxidation after reduction, they were stored in sealed vials with an inert solvent; moreover, samples were prepared in a dry box under a N2 flow, where the solvent was evaporated prior to its introduction into the analysis chamber, and directly analyzed without previous treatment.
To calculate the total acid sites present in the samples, thermo-programmed desorption of ammonia (NH3-TPD) was carried out. In a typical procedure, 0.08 g of catalyst is placed in a U-shape quartz reactor and cleaned flowing He (40 mL·min−1) up to 400 °C with a heating rate of 10 °C·min−1. Then, the sample is cooled until 100 °C under the same He flow, and once the temperature is stabilized at 100 °C, the sample is saturated with ammonia for 5 minutes and then physisorbed NH3 was removed under He. Ammonia desorption is performed by heating the sample from 100 to 400 °C, with a rate of 10 °C·min−1, registering the signal using a GC-14B instrument (Shimadzu, Kioto, Japan) equipped with a thermal conductivity detector (TCD), previously calibrated with Ni(NH3)6Cl2 (Aldrich) in order to quantify total acid sites.
Thermo-programmed desorption of CO2 (CO2-TPD) was employed for the quantification of basic sites. In a typical procedure, 0.03 g of catalyst is pretreated under a He flow (40 mL min−1) at 400 °C for 15 min (10 °C·min−1). Later, the sample was cooled to 100 °C and a pure CO2 stream (60 mL min−1) was subsequently introduced into the reactor for 30 min. Finally, the amount of CO2 evolved was analyzed using a TCD detector between 100 and 600 °C and a helium flow (10 °C min−1).

4.3. Catalytic Tests

The furfural hydrogenation was carried out at atmospheric pressure in a tubular quartz reactor with an internal diameter of 6.35 mm. For this, 150 mg of pelletized catalyst (325–400 μm) were placed inside the reactor between two layers of quartz wool, which is placed inside a programmable temperature tubular furnace, controlled with a thermocouple. Before starting the reaction, catalysts were reduced in-situ with a hydrogen flow (99.99%, Airgas, Paris, France) of 60 mL min−1 for 1 h at the reduction temperature deduced from their corresponding H2-TPR profiles (350 °C). Subsequently, the desired reaction temperature is set and once the system is stable, the reaction is carried out under a flow of H2 that ranges between 10 and 60 ml min−1 and a feed flow of 3.87 mL h−1 of a furfural solution in cyclopentyl methyl ether (CPME, 5 vol.%), which is introduced with the help of an HPLC piston pump, model 307 SC-10 (Gilson, Middleton, WI, USA).
To avoid problems, such as blockage of the lines in the equipment, furfural was dissolved in cyclopentyl methyl ether (CPME). This solvent is environmentally friendly and has been used in different organic reactions [30]. Reaction samples were collected every hour, dissolved with a chloroform and o-xylene solution (internal standard), stored in sealed vials to be subsequently analyzed by gas chromatography, using a Shimazu GB-14A chromatograph equipped with a flame ionization detector and a CP-Wax 52 CB capillary column.
In a preliminary test, the CuZn_1 catalyst was chosen to evaluate the stability of this solvent at 190 °C, after 5 h of time-on-stream (TOS), but in the absence of furfural. The analysis of the collected samples confirmed the full recovery of CPME; without any products different from this ether, thus demonstrating its stability. The conversion, selectivity and yield values were determined using the following expressions:
Conversion   ( % ) = mol   of   furfural   converted mol   of   furfural   fed × 100
Selectivity   ( % ) = mol   of   the   product mol   of   furfural   converted × 100
Yield   ( % ) = mol   of   the   product mol   of   furfural   fed × 100
The turnover frequency was calculated as follows (6):
TOF = ln   ( 1 X ) ( W F ) × M
where F is the molar rate of furfural (mol h−1), W is the catalyst weight (g), X is the conversion and M is the mole of sites loaded (mol g−1). This equation, in which –ln (1 − X) substitutes for X assumes a pseudo first-order reaction which may be justified by the excess of hydrogen [63].

5. Conclusions

Several LDHs with chemical composition (Cu,Zn)1−xAlx(OH)2(CO3)x/2·mH2O have been synthesized by the co-precipitation method, maintaining a (Cu2+ + Zn2+)/Al3+ molar ratio of 3, and varying the Cu2+/Zn2+ molar ratio between 0.2 and 6.0. After calcination and reduction steps, Cu/ZnO/Al2O3 catalysts were obtained. The physico-chemical characterization has revealed the formation of small Cu nanoparticles highly dispersed in the ZnO-Al2O3 structure.
All the catalysts were active in the gas-phase hydrogenation of furfural, with a high selectivity toward furfuryl alcohol, which is considered a valuable product due to its use for manufacturing resins. The presence of a low proportion of acid sites seems to disfavor consecutive reactions, being the formation of MF very limited in all cases. In addition, the textural properties of catalysts are typical of meso- and mainly macroporous solids, and the weaker Cu0-FUR interaction, in comparison to other supports with stronger acidity, favors the lability of adsorbed reaction products and consequently shorter residence times, minimizing the deactivation by the formation of carbonaceous deposits.
In additional studies, the influence of the aging time in the synthesis of LDHs was also evaluated. The catalytic results have demonstrated that a shorter aging time leads to the formation of catalyst with a lower crystallinity, which favors the formation of Cu0-rich surfaces. This provides more active and stable catalysts, highly selective to FOL, obtaining a maximum FOL yield of 71% after 5 h of TOS at 210 °C for the CuZn_1 catalyst that was aged for 1 h.

Author Contributions

Conceptualization: J.A.C. and P.M.-T.; methodology: C.P.J.-G. and J.A.C.; validation: C.P.J.-G, J.A.C. and P.M.-T; formal analysis: G.R.B. and C.P.J.-G.; investigation: G.R.B. and C.P.J.-G.; resources: P.M.-T; data curation: C.P.J.-G. and J.A.C.; writing—original draft preparation: J.A.C.; writing—review and editing: C.P.J.-G., J.A.C. and P.M.-T.; visualization: C.P.J.-G. and J.A.C.; supervision: J.A.C. and P.M.-T.; project administration: P.M.-T.; funding acquisition: P.M.-T. All authors have read and agreed to the published version of the manuscript.

Funding

The authors are grateful to financial support from the Spanish Ministry of Innovation, Science and Universities (Project RTI2018- 094918-B-C44) and FEDER (European Union) funds.

Acknowledgments

J.A.C. and C.P.J.-G. thank University of Malaga for contracts of PhD incorporation.

Conflicts of Interest

The authors declare that they have no known competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

References

  1. Cavanni, F.; Trifiró, F.; Vaccari, A. Hydrotalcite-type anionic clays: Preparation, properties and applications. Catal. Today 1991, 11, 173–301. [Google Scholar] [CrossRef]
  2. Mishra, G.; Dash, B.; Pandey, S. Layered double hydroxides: A brief review from fundamentals to application as evolving biomaterials. Appl. Clay Sci. 2018, 153, 172–186. [Google Scholar] [CrossRef]
  3. Bukhtiyarova, M.V. A review on effect of synthesis conditions on the formation of layered double hydroxides. J. Solid State Chem. 2019, 269, 494–506. [Google Scholar] [CrossRef]
  4. Kuthati, Y.; Kankala, R.K.; Lee, C.H. Layered double hydroxide nanoparticles for biomedical applications: Current status and recent prospects. Appl. Clay Sci. 2015, 112, 100–116. [Google Scholar] [CrossRef]
  5. Constantino, V.R.L.; Pinnavaia, T.J. Structure-reactivity relationships for basic catalysts derived from a Mg2+/A13+/CO3− layered double hydroxide. Catal. Lett. 1994, 23, 361–367. [Google Scholar] [CrossRef]
  6. Prinetto, F.; Ghiotti, G.; Durand, R.; Tichit, D. Investigation of acid-base properties of catalysts obtained from layered double hydroxides. J. Phys. Chem. B 2000, 104, 11117–11126. [Google Scholar] [CrossRef]
  7. Corma Canos, A.; Iborra, S.; Velty, A. Chemical routes for the transformation of biomass into chemicals. Chem. Rev. 2007, 107, 2411–2502. [Google Scholar] [CrossRef]
  8. Climent, M.J.; Corma, A.; Iborra, S. Conversion of biomass platform molecules into fuel additives and liquid hydrocarbon fuels. Green Chem. 2014, 16, 516–547. [Google Scholar] [CrossRef] [Green Version]
  9. Binder, J.B.; Raines, R.T. Simple chemical transformation of lignocellulosic biomass into furans for fuels and chemicals. J. Am. Chem. Soc. 2009, 131, 1979–1985. [Google Scholar] [CrossRef]
  10. Alonso, D.M.; Wettstein, S.G.; Mellmer, M.A.; Gurbuz, E.I.; Dumesic, J.A. Integrated conversion of hemicellulose and cellulose from lignocellulosic biomass. Energy Environ. Sci. 2013, 6, 76–80. [Google Scholar] [CrossRef]
  11. Delbecq, F.; Wang, Y.; Muralidhara, A.; El Ouardi, K.E.; Marlair, G.; Len, C. Hydrolysis of hemicellulose and derivatives-a review of recent advances in the production of furfural. Front. Chem. 2018, 6, 146–175. [Google Scholar] [CrossRef]
  12. Mariscal, R.; Maireles-Torres, P.; Ojeda, M.; Sádaba, I.; López Granados, M. Furfural: A renewable and versatile platform molecule for the synthesis of chemicals and fuels. Energy Environ. Sci. 2016, 9, 1144–1189. [Google Scholar] [CrossRef]
  13. Fúnez-Núñez, I.; García-Sancho, C.; Cecilia, J.A.; Moreno-Tost, R.; Pérez-Inestrosa, E.; Serrano-Cantador, L.; Maireles-Torres, P. Synergistic effect between CaCl2 and γ-Al2O3 for furfural production by dehydration of hemicellulosic carbohydrates. Appl. Catal. A Gen. 2019, 585, 117188. [Google Scholar] [CrossRef]
  14. Zeitsch, K.J. The Chemistry and Technology of Furfural and Its Many By-Products; Elsevier Science: New York, NY, USA, 2000. [Google Scholar]
  15. Yan, K.; Wu, G.; Lafleur, T.; Jarvis, C. Production, properties and catalytic hydrogenation of furfural to fuel additives and value-added chemicals. Renew. Sustain. Energy Rev. 2014, 38, 663–676. [Google Scholar] [CrossRef]
  16. Ramesh, D.; Reddy, T.S.; Narasimhulu, M.; Rajaram, S.; Suryakiran, N.; Mahesh, K.C.; Venkateswarlu, Y. Efficient and rapid stereoselective synthesis of trans-4,5-diaminocyclopent-2-enones by acidic ionic liquid under solvent-free conditions. Chem. Lett 2009, 38, 586–587. [Google Scholar] [CrossRef]
  17. Nardi, M.; Costanzo, P.; de Nino, A.; di Gioia, M.L.; Olivito, F.; Sindona, G.; Procopio, A. Water excellent solvent for the synthesis of bifunctionalized cyclopentenones from furfural. Green Chem. 2017, 19, 5403–5411. [Google Scholar] [CrossRef]
  18. Guo, J.; Xu, G.; Han, Z.; Zhang, Y.; Fu, Y.; Guo, Q. Selective conversion of furfural to cyclopentanone with CuZnAl catalysts. ACS Sustain. Chem. Eng. 2014, 2, 2259–2266. [Google Scholar] [CrossRef]
  19. Li, S.W.; Batey, R.A. Mild lanthanide(iii) catalyzed formation of 4,5-diaminocyclopent-2-enones from 2-furaldehyde and secondary amines: A domino condensation/ring-opening/electrocyclization process. Chem. Commun. 2007, 3759–3761. [Google Scholar] [CrossRef]
  20. Procopio, A.; Costanzo, P.; Curini, M.; Nardi, M.; Oliveiro, M.; Sindona, G. Erbium(III) Chloride in ethyl lactate as a smart ecofriendly system for efficient and rapid stereoselective synthesis of trans-4,5-diaminocyclopent-2-enones. ACS Sustain. Chem. Eng. 2013, 1, 541–544. [Google Scholar] [CrossRef]
  21. Burnett, L.W.; Johns, I.B.; Holdren, R.F.; Hixon, R.M. Production of 2-Methylfuran by Vapor-Phase Hydrogenation of Furfural. Ind. Eng. Chem. 1948, 40, 502–505. [Google Scholar] [CrossRef]
  22. Manly, D.; Dunlop, A.P. Catalytic Hydrogenation. I. Kinetics and catalyst composition in the preparation of 2-methylfuran. J. Org. Chem. 1958, 23, 1093–1095. [Google Scholar] [CrossRef]
  23. Seo, G.; Chon, H. Hydrogenation of furfural over copper-containing catalysts. J. Catal. 1981, 67, 424–429. [Google Scholar] [CrossRef]
  24. Rao, R.; Dandekar, A.; Baker, R.T.K.; Vannice, M.A. Properties of Copper Chromite Catalysts in Hydrogenation Reactions. J. Catal. 1997, 171, 406–419. [Google Scholar] [CrossRef]
  25. Nagaraja, B.M.; Siva Kumar, V.; Shasikala, V.; Padmasri, A.H.; Sreedhar, B.; David Raju, B.; Rama Rao, K.S. A highly efficient Cu/MgO catalyst for vapour phase hydrogenation of furfural to furfuryl alcohol. Catal. Commun. 2003, 4, 287–293. [Google Scholar] [CrossRef]
  26. Nagaraja, B.M.; Padmasri, A.H.; David Raju, B.; Rama Rao, K.S. Vapor phase selective hydrogenation of furfural to furfuryl alcohol over Cu-MgO coprecipitated catalysts. J. Mol. Catal. A Chem. 2007, 265, 90–97. [Google Scholar] [CrossRef]
  27. Sitthisa, S.; Sooknoi, T.; Ma, Y.; Balbuena, P.B.; Resasco, D.E. Kinetics and mechanism of hydrogenation of furfural on Cu/SiO2 catalysts. J. Catal. 2011, 277, 1–13. [Google Scholar] [CrossRef]
  28. Sitthisa, S.; Resasco, D.E. Hydrodeoxygenation of Furfural Over Supported Metal Catalysts: A Comparative Study of Cu, Pd and Ni. Catal. Lett. 2011, 141, 784–791. [Google Scholar] [CrossRef]
  29. Dong, F.; Zhu, Y.; Zheng, H.; Zhu, Y.; Li, X.; Li, Y. Cr-free Cu-catalysts for the selective hydrogenation of biomass-derived furfural to 2-methylfuran: The synergistic effect of metal and acid sites. J. Mol. Catal. A Chem. 2015, 398, 140–148. [Google Scholar] [CrossRef]
  30. Jiménez-Gómez, C.P.; Cecilia, J.A.; Durán-Martín, D.; Moreno-Tost, R.; Santamaría-González, J.; Mérida-Robles, J.; Mariscal, R.; Maireles-Torres, P. Gas-phase hydrogenation of furfural to furfuryl alcohol over Cu/ZnO catalysts. J. Catal. 2016, 336, 107–115. [Google Scholar] [CrossRef]
  31. Ghashghaee, M.; Sadjadi, S.; Shirvani, S.; Farzaneh, V. A Novel Consecutive Approach for the Preparation of Cu–MgO Catalysts with High Activity for Hydrogenation of Furfural to Furfuryl Alcohol. Catal. Lett. 2017, 147, 318–327. [Google Scholar] [CrossRef]
  32. Jiménez-Gómez, C.P.; Cecilia, J.A.; Moreno-Tost, R.; Maireles-Torres, P. Selective Production of 2-Methylfuran by Gas-Phase Hydrogenation of Furfural on Copper Incorporated by Complexation in Mesoporous Silica Catalysts. ChemSusChem 2017, 10, 1448–1459. [Google Scholar] [CrossRef] [PubMed]
  33. Jiménez-Gómez, C.P.; Cecilia, J.A.; Moreno-Tost, R.; Maireles-Torres, P. Selective Furfural Hydrogenation to Furfuryl Alcohol Using Cu-Based Catalysts Supported on Clay Minerals. Top. Catal. 2017, 60, 1040–1053. [Google Scholar] [CrossRef]
  34. Yang, X.; Chen, H.; Meng, Q.; Zheng, H.; Zhu, Y.; Li, Y.W. Insights into influence of nanoparticle size and metal-support interactions of Cu/ZnO catalysts on activity for furfural hydrogenation. Catal. Sci. Technol. 2017, 7, 5625–5634. [Google Scholar] [CrossRef]
  35. Sulmonetti, T.P.; Pang, S.H.; Claure, M.T.; Lee, S.; Cullen, D.A.; Agrawal, P.K.; Jones, C.W. Vapor phase hydrogenation of furfural over nickel mixed metal oxide catalysts derived from layered double hydroxides. Appl. Catal. A Gen. 2016, 517, 187–195. [Google Scholar] [CrossRef] [Green Version]
  36. Manikandan, M.; Venugopal, A.K.; Prabu, K.; Jha, R.K.; Thirumalaiswamy, R. Role of surface synergistic effect on the performance of Ni-based hydrotalcite catalyst for highly efficient hydrogenation of furfural. J. Mol. Catal. A Chem. 2016, 417, 153–162. [Google Scholar] [CrossRef]
  37. Guerrero-Torres, A.; Jiménez-Gómez, C.P.; Cecilia, J.A.; García-Sancho, C.; Quirante-Sánchez, J.J.; Mérida-Robles, J.M.; Maireles-Torres, P. Influence of the incorporation of basic or amphoteric oxides on the performance of Cu-based catalysts supported on sepiolite in furfural hydrogenation. Catalysts 2019, 9, 315. [Google Scholar] [CrossRef] [Green Version]
  38. Nakagawa, Y.; Nakazawa, H.; Watanabe, H.; Tomishige, K. Total Hydrogenation of Furfural over a Silica-Supported Nickel Catalyst Prepared by the Reduction of a Nickel Nitrate Precursor. ChemCatChem 2012, 4, 1791–1797. [Google Scholar] [CrossRef]
  39. Jiménez-Gómez, C.P.; Cecilia, J.A.; Moreno-Tost, R.; Maireles-Torres, P. Nickel Phosphide/Silica Catalysts for the Gas-Phase Hydrogenation of Furfural to High–Added–Value Chemicals. ChemCatChem 2017, 9, 2881–2889. [Google Scholar] [CrossRef]
  40. Jiménez-Gómez, C.P.; Cecilia, J.A.; García-Sancho, C.; Moreno-Tost, R.; Maireles-Torres, P. Selective Production of Furan from Gas-Phase Furfural Decarbonylation on Ni-MgO Catalysts. ACS Sustain. Chem. Eng. 2019, 7, 7676–7685. [Google Scholar] [CrossRef]
  41. Guerrero-Torres, A.; Jiménez-Gómez, C.P.; Cecilia, J.A.; García-Sancho, C.; Franco, F.; Quirante-Sánchez, J.J.; Maireles-Torres, P. Ni supported on sepiolite catalysts for the hydrogenation of furfural to value-added chemicals: Influence of the synthesis method on the catalytic performance. Top. Catal. 2019, 62, 535–550. [Google Scholar] [CrossRef]
  42. Sitthisa, S.; Pham, T.; Prasomsri, T.; Sooknoi, T.; Mallinson, R.G.; Resasco, D.E. Conversion of furfural and 2-methylpentanal on Pd/SiO2 and Pd-Cu/SiO2 catalysts. J. Catal. 2011, 280, 17–27. [Google Scholar] [CrossRef]
  43. Pino, N.; Sitthisa, S.; Tan, Q.; Souza, T.; López, D.; Resasco, D.E. Structure, activity, and selectivity of bimetallic Pd-Fe/SiO2 and Pd-Fe/γ-Al2O3 catalysts for the conversion of furfural. J. Catal. 2017, 350, 30–40. [Google Scholar] [CrossRef] [Green Version]
  44. Yang, X.; Meng, Q.; Ding, G.; Wang, Y.; Chen, H.; Zhu, Y.L.; Li, Y.W. Construction of novel Cu/ZnO-Al2O3 composites for furfural hydrogenation: The role of Al components. Appl. Catal. A Gen. 2018, 561, 78–86. [Google Scholar] [CrossRef]
  45. Nogueira, K.A.B.; Cecilia, J.A.; Santos, S.O.; Aguiar, J.E.; Vilarrasa-García, E.; Rodríguez-Castellón, E.; Azevedo, D.C.S.; Silva, I.J. Adsorption behavior of bovine serum albumin on Zn–Al and Mg–Al layered double hydroxides. J. Sol-Gel Sci. Technol. 2016, 80, 748–758. [Google Scholar] [CrossRef]
  46. Santos, J.L.; Reina, T.R.; Ivanova, S.; Centeno, M.A.; Odriozola, J.A. Gold promoted Cu/ZnO/Al2O3 catalysts prepared from hydrotalcite precursors: Advanced materials for the WGS reaction. Appl. Catal. B Environ. 2017, 201, 310–317. [Google Scholar] [CrossRef]
  47. He, L.; Cheng, H.; Liang, G.; Yu, Y.; Zhao, F. Effect of structure of CuO/ZnO/Al2O3 composites on catalytic performance for hydrogenation of fatty acid ester. Appl. Catal. A Gen. 2013, 452, 88–93. [Google Scholar] [CrossRef]
  48. Fierro, J.L.G.; Melián-Cabrera, I.; López Granados, M. Reverse topotactic transformation of a Cu-Zn-Al catalyst during wet Pd impregnation: Relevance for the performance in methanol synthesis from CO2/H2 mixtures. J. Catal. 2002, 210, 273–284. [Google Scholar]
  49. Chinchen, G.C.; Waugh, K.C.; Whan, D.A. The activity and state of the copper surface in methanol synthesis catalysts. Appl. Catal. 1986, 25, 101–107. [Google Scholar] [CrossRef]
  50. Gervasini, A.; Bennici, S. Dispersion and surface states of copper catalysts by temperature-programmed-reduction of oxidized surfaces (s-TPR). Appl. Catal. A Gen. 2005, 281, 199–205. [Google Scholar] [CrossRef]
  51. Yahiro, H.; Nakaya, K.; Yamamoto, T.; Saiki, K.; Yamaura, H. Effect of calcination temperature on the catalytic activity of copper supported on γ-alumina for the water-gas-shift reaction. Catal. Commun. 2006, 7, 228–231. [Google Scholar] [CrossRef]
  52. Williamson, G.K.; Hall, W.H. X-ray line broadening line from filed aluminium and wolfram. Acta Metall. 1953, 1, 22–31. [Google Scholar] [CrossRef]
  53. Studt, F.; Abild-Pedersen, F.; Varley, J.B.; Nørskov, J.K. CO and CO2 hydrogenation to methanol calculated using the BEEF-vdW functional. Catal. Lett. 2013, 143, 71–73. [Google Scholar] [CrossRef] [Green Version]
  54. Maderuelo-Solera, R.; López-Asensio, R.; Cecilia, J.A.; Jiménez-Gómez, C.P.; García-Sancho, C.; Moreno-Tost, R.; Maireles-Torres, P. Catalytic transfer hydrogenation of furfural to furfuryl alcohol over calcined MgFe hydrotalcites. Appl. Clay Sci. 2019, 183, 105351–105363. [Google Scholar] [CrossRef]
  55. Thommes, M.; Kaneko, K.; Neimark, A.V.; Olivier, J.P.; Rodriguez-Reinoso, F.; Rouquerol, J.; Sing, K.S.W. Physisorption of gases, with special reference to the evaluation of surface area and pore size distribution (IUPAC Technical Report). Pure Appl. Chem. 2015, 87, 1051–1069. [Google Scholar] [CrossRef] [Green Version]
  56. Landers, J.; Gor, G.Y.; Neimark, A.V. Density functional theory methods for characterization of porous materials. Colloids Surfaces A Physicochem. Eng. Asp. 2013, 437, 3–32. [Google Scholar]
  57. Pakharukova, V.P.; Moroz, E.M.; Zyuzin, D.A.; Ishchenko, A.V.; Dolgikh, L.Y.; Strizhak, P.E. Structure of Copper Oxide Species Supported on Monoclinic Zirconia. J. Phys. Chem. C 2015, 119, 28828–28835. [Google Scholar]
  58. Arango-Díaz, A.; Cecilia, J.A.; Dos Santos-Gómez, L.; Marrero-López, D.; Losilla, E.R.; Jiménez-Jiménez, J.; Rodríguez-Castellón, E. Characterization and performance in preferential oxidation of CO of CuO-CeO2 catalysts synthesized using polymethyl metacrylate (PMMA) as template. Int. J. Hydrog. Energy 2015, 40, 11254–11260. [Google Scholar]
  59. Kattel, S.; Ramírez, P.J.; Chen, J.G.; Rodriguez, J.A.; Liu, P. Active sites for CO2 hydrogenation to methanol on Cu/ZnO catalysts. Science (80-.) 2017, 355, 1296–1299. [Google Scholar] [CrossRef] [Green Version]
  60. Peplinski, B.; Unger, W.E.S.; Grohmann, I. Characterization of CuZnAl oxide catalysts in the precipitaed, calcined and reduced state by means of XPS with the help of a finger-print data base. Appl. Surf. Sci. 1992, 62, 115–129. [Google Scholar] [CrossRef]
  61. Moulder, J.F.; Stickle, W.F.; Sool, P.E.; Bomber, K.D. Handbook of X-ray Photoelectron Spectroscopy; Pekin-Elmer: Eden Praire, NM, USA, 1992. [Google Scholar]
  62. Liu, D.; Zemlyanov, D.; Wu, T.; Lobo-Lapidus, R.J.; Dumesic, J.A.; Miller, J.T.; Marshall, C.L. Deactivation mechanistic studies of copper chromite catalyst for selective hydrogenation of 2-furfuraldehyde. J. Catal. 2013, 299, 336–345. [Google Scholar] [CrossRef]
  63. Jiménez-Gómez, C.P.; Cecilia, J.A.; Márquez-Rodríguez, I.; Moreno-Tost, R.; Santamaría-González, J.; Mérida-Robles, J.; Maireles-Torres, P. Gas-phase hydrogenation of furfural over Cu/CeO2 catalysts. Catal. Today 2017, 279, 327–338. [Google Scholar] [CrossRef]
  64. Wu, J.; Shen, Y.; Liu, C.; Wang, H.; Geng, C.; Zhang, Z. Vapor phase hydrogenation of furfural to furfuryl alcohol over environmentally friendly Cu-Ca/SiO2 catalyst. Catal. Commun. 2005, 6, 633–637. [Google Scholar] [CrossRef]
  65. Solinas, V.; Ferino, I. Microcalorimetric characterisation of acid-basic catalysts. Catal. Today 1998, 41, 179–189. [Google Scholar] [CrossRef]
  66. Gervasini, A.; Auroux, A. Microcalorimetric investigation of the acidity and basicity of metal oxides. J. Therm. Anal. 1991, 37, 1737–1744. [Google Scholar] [CrossRef]
  67. Watanabe, K.; Yamagiwa, N.; Torisawa, Y. Cyclopentyl methyl ether as a new and alternative process solvent. Org. Process Res. Dev. 2007, 11, 251–258. [Google Scholar] [CrossRef]
  68. Shi, Y.; Zhu, Y.; Yang, Y.; Li, Y.W.; Jiao, H. Exploring Furfural Catalytic Conversion on Cu(111) from Computation. ACS Catal. 2015, 5, 4020–4032. [Google Scholar] [CrossRef]
  69. Pillai, U.R.; Deevi, S. Copper-zinc oxide and ceria promoted copper-zinc oxide as highly active catalysts for low temperature oxidation of carbon monoxide. Appl. Catal. B Environ. 2006, 65, 110–117. [Google Scholar] [CrossRef]
  70. Jiménez-Gómez, C.P.; Cecilia, J.A.; Franco-Duro, F.I.; Pozo, M.; Moreno-Tost, R.; Maireles-Torres, P. Promotion effect of Ce or Zn oxides for improving furfuryl alcohol yield in the furfural hydrogenation using inexpensive Cu-based catalysts. Mol. Catal. 2018, 455, 121–131. [Google Scholar] [CrossRef]
  71. Abderrazek, K.; Frini Srasra, N.; Srasra, E. Synthesis and Characterization of [Zn-Al] Layered Double Hydroxides: Effect of the Operating Parameters. J. Chin. Chem. Soc. 2017, 64, 346–353. [Google Scholar] [CrossRef]
  72. Brunauer, S.; Emmett, P.H.; Teller, E. Adsorption of Gases in Multimolecular Layers. J. Am. Chem. Soc. 1938, 60, 309–319. [Google Scholar] [CrossRef]
Figure 1. XRD patterns of the layered double CuZnAl hydroxides. (Circles: zinc hydroxycarbonate), (diamonds: copper(II) hydroxide).
Figure 1. XRD patterns of the layered double CuZnAl hydroxides. (Circles: zinc hydroxycarbonate), (diamonds: copper(II) hydroxide).
Catalysts 10 00486 g001
Figure 2. XRD profiles of the mixed oxides obtained after the calcination of LDHs at 300 °C.
Figure 2. XRD profiles of the mixed oxides obtained after the calcination of LDHs at 300 °C.
Catalysts 10 00486 g002
Figure 3. H2-TPR profiles of the mixed metal oxides obtained after calcination of LDHs.
Figure 3. H2-TPR profiles of the mixed metal oxides obtained after calcination of LDHs.
Catalysts 10 00486 g003
Figure 4. XRD patterns of the CuZn_X catalysts.
Figure 4. XRD patterns of the CuZn_X catalysts.
Catalysts 10 00486 g004
Figure 5. TEM micrographs for CuZn_0.2, CuZn_1 and CuZn_6. (Scale bar: 50 nm).
Figure 5. TEM micrographs for CuZn_0.2, CuZn_1 and CuZn_6. (Scale bar: 50 nm).
Catalysts 10 00486 g005
Figure 6. EDX images of CuZn_0.2, CuZn_1 and CuZn_6. (Scale bar: 200 nm).
Figure 6. EDX images of CuZn_0.2, CuZn_1 and CuZn_6. (Scale bar: 200 nm).
Catalysts 10 00486 g006
Figure 7. N2 adsorption-desorption isotherms at −196 °C (A) and pore size distribution estimated by DFT method (B) for CuZn_X catalysts.
Figure 7. N2 adsorption-desorption isotherms at −196 °C (A) and pore size distribution estimated by DFT method (B) for CuZn_X catalysts.
Catalysts 10 00486 g007
Figure 8. Cu 2p core level (A), Auger CuLMM (B) and Auger ZnLMM (C) spectra of CuZn_X catalysts.
Figure 8. Cu 2p core level (A), Auger CuLMM (B) and Auger ZnLMM (C) spectra of CuZn_X catalysts.
Catalysts 10 00486 g008
Figure 9. FUR conversion (A), FOL yield (B), and MF yield (C) in the FUR hydrogenation over CuZn_X catalysts (Experimental conditions: Mass of catalyst = 0.15 g, Reaction temperature = 190 °C, Pressure = 0.1 MPa, H2 flow = 10 mL min−1, Fed flow = 2.3 mmol FUR h−1).
Figure 9. FUR conversion (A), FOL yield (B), and MF yield (C) in the FUR hydrogenation over CuZn_X catalysts (Experimental conditions: Mass of catalyst = 0.15 g, Reaction temperature = 190 °C, Pressure = 0.1 MPa, H2 flow = 10 mL min−1, Fed flow = 2.3 mmol FUR h−1).
Catalysts 10 00486 g009
Figure 10. Linearization of TOF values (A) and FUR consumption rate (B) with time-on-stream for CuZn_X catalysts.
Figure 10. Linearization of TOF values (A) and FUR consumption rate (B) with time-on-stream for CuZn_X catalysts.
Catalysts 10 00486 g010
Figure 11. FUR conversion (A), FOL yield (B), and MF yield (C) in the FUR hydrogenation with CuZn_6 (Experimental conditions: Mass of catalyst = 0.15 g, Pressure = 0.1 MPa, H2 flow = 10 mL min−1, Fed flow = 2.3 mmol FUR h−1).
Figure 11. FUR conversion (A), FOL yield (B), and MF yield (C) in the FUR hydrogenation with CuZn_6 (Experimental conditions: Mass of catalyst = 0.15 g, Pressure = 0.1 MPa, H2 flow = 10 mL min−1, Fed flow = 2.3 mmol FUR h−1).
Catalysts 10 00486 g011
Figure 12. FUR conversion (A), FOL yield (B), and MF yield (C) in the FUR hydrogenation over CuZn_1 catalysts synthesized with different aging time (1–168 h) (Experimental conditions: Mass of catalyst = 0.15 g, Pressure = 0.1 MPa, H2 flow = 10 mL min−1, Fed flow = 2.3 mmol FUR h−1).
Figure 12. FUR conversion (A), FOL yield (B), and MF yield (C) in the FUR hydrogenation over CuZn_1 catalysts synthesized with different aging time (1–168 h) (Experimental conditions: Mass of catalyst = 0.15 g, Pressure = 0.1 MPa, H2 flow = 10 mL min−1, Fed flow = 2.3 mmol FUR h−1).
Catalysts 10 00486 g012
Figure 13. XRD (A) and H2-TPR (B) profiles of CuZn_1 catalysts synthesized with different aging time.
Figure 13. XRD (A) and H2-TPR (B) profiles of CuZn_1 catalysts synthesized with different aging time.
Catalysts 10 00486 g013aCatalysts 10 00486 g013b
Table 1. Chemical composition and H2 consumption of mixed metal oxides obtained by calcination of LDHs.
Table 1. Chemical composition and H2 consumption of mixed metal oxides obtained by calcination of LDHs.
CatalystContent (wt.%)Deconvolution H2-TPR (%)H2 Consumption (μmol g−1)
CuZnOAl2O3Peak 1Peak 2ExperimentalTheoretical
CuZn_0.211.171.117.8683215161696
CuZn_0.419.462.318.2594127632921
CuZn_135.645.519.0386248685131
CuZn_2.553.027.219.959568237356
CuZn_665.614.020.529883768857
Table 2. Textural properties of the CuZn_X catalysts.
Table 2. Textural properties of the CuZn_X catalysts.
CatalystSBET (m2 g−1)t-Plot (m2 g−1)Pore Volume (cm3 g−1)Micropore Volume 1 (cm3 g−1)Amount Acid Sites 2 (μmol g−1)Amount Basic Sites 3 (μmol g−1)
CuZn_0.28550.4740.0027839
CuZn_0.47960.5900.0037631
CuZn_17910.6070.0016922
CuZn_2.58490.6790.0055917
CnZn_67080.5330.0036015
1 Micropore volume estimated from alpha-s-plot. 2 Quantification of acid sites by NH3-TPD. 3 Quantification of acid sites by CO2-TPD.
Table 3. Metallic properties of CuZn_X catalysts, as determined from N2O titration.
Table 3. Metallic properties of CuZn_X catalysts, as determined from N2O titration.
CatalystSuperficial H2 UptakeMetallic SurfaceDispersionParticle SizeCrystallite Size 1
(μmol g−1)(m2Cu gCu−1)(m2Cu gcat−1)(%)(nm)(nm)
CuZn_0.2317118132155
CuZn_0.438582161486
CuZn_14755519101215
CuZn_2.5563442381521
CuZn_6555352371929
1 By applying the Williamson-Hall equation to XRD data [52].
Table 4. XPS data of CuZn_X catalysts.
Table 4. XPS data of CuZn_X catalysts.
CatalystBinding Energy, eV (Atomic Concentration, %)Surface Molar Ratio
C 1sO 1sAl 2pCu 2pZn 2pCu/Zn(Cu + Zn)/Al
CuZn_0.2284.8288.7531.1532.774.4932.01022.10.152.37
(9.6)(1.6)(46.2)(5.8)(10.9)(3.7)(22.1)
CuZn_0.4284.8288.8530.8532.574.3932.11021.90.292.16
(16.6)(0.9)(40.7)(13.0)(9.1)(4.5)(15.2)
CuZn_1284.8288.6531.0532.674.4932.11022.10.511.97
(10.1)(1.0)(38.6)(14.1)(12.2)(8.1)(16.0)
CuZn_2.5284.8288.4531.0532.774.5932.01022.10.831.88
(14.1)(0.7)(36.7)(15.3)(11.5)(9.8)(11.8)
CuZn_6284.8288.4531.0532.574.5932.01021.71.831.77
(17.4)(1.1)(37.9)(8.7)(9.6)(11.0)(6.0)
Table 5. Turnover frequency and lifetime analysis of CuZn_X catalysts, obtained from linearization of Figure 10.
Table 5. Turnover frequency and lifetime analysis of CuZn_X catalysts, obtained from linearization of Figure 10.
CatalystTOF0 1 (h−1)C0 2 (%)r0 3 (mmolFUR h−1 g−1)Exhaustion Time 4 (h)Total FUR Converted 5 (mmolFUR g−1)FUR Converted (1–5 h) 6 (mmolFUR g−1)
CuZn_0.228430.6748·10−210.00.04400.0201
CuZn_0.443580.9105·10−213.40.09160.0307
CuZn_144721.1352·10−215.20.15370.0402
CuZn_2.536761.1897·10−29.90.09960.0366
CuZn_637731.1410·10−210.00.10210.0369
1 Turnover frequency determined at t0 (metallic surface data were obtained from Table 3). 2 Conversion of FUR at t0. 3 FUR rates at t0. 4 Total exhaustion time of catalysts. 5 Total FUR converted until catalyst exhaustion. 6 FUR converted between 1 and 5 h of TOS.
Table 6. Metallic characteristic of CuZn_1 catalysts synthesized with different aging time. determined from N2O titration.
Table 6. Metallic characteristic of CuZn_1 catalysts synthesized with different aging time. determined from N2O titration.
CatalystSuperficial H2-UptakeMetallic SurfaceD 1Particle SizeCrystal Size 2
(μmol g−1)(m2Cu gCu−1)(m2Cu gcat−1)(%)(nm)(nm)
CuZn_1(1h)5956924129-
CuZn_1(48h)4755519101215
CuZn_1(168h)307361261933
1 Copper dispersion. 2 Crystal size estimated by Williamson-Hall equation from XRD data [52].
Table 7. Surface atomic concentration of CuZn_1 catalysts synthesized with different aging time.
Table 7. Surface atomic concentration of CuZn_1 catalysts synthesized with different aging time.
CatalystAtomic Concentration (%)
C 1sO 1sAl 2pCu 2pZn 2p
CuZn_1(1h)11.0152.8311.958.3515.86
CuZn_1(48h)11.0652.7112.218.0715.99
CuZn_1(196h)15.4650.7010.876.7116.26

Share and Cite

MDPI and ACS Style

R. Bertolini, G.; Jiménez-Gómez, C.P.; Cecilia, J.A.; Maireles-Torres, P. Gas-Phase Hydrogenation of Furfural to Furfuryl Alcohol over Cu-ZnO-Al2O3 Catalysts Prepared from Layered Double Hydroxides. Catalysts 2020, 10, 486. https://doi.org/10.3390/catal10050486

AMA Style

R. Bertolini G, Jiménez-Gómez CP, Cecilia JA, Maireles-Torres P. Gas-Phase Hydrogenation of Furfural to Furfuryl Alcohol over Cu-ZnO-Al2O3 Catalysts Prepared from Layered Double Hydroxides. Catalysts. 2020; 10(5):486. https://doi.org/10.3390/catal10050486

Chicago/Turabian Style

R. Bertolini, Guillermo, Carmen P. Jiménez-Gómez, Juan Antonio Cecilia, and Pedro Maireles-Torres. 2020. "Gas-Phase Hydrogenation of Furfural to Furfuryl Alcohol over Cu-ZnO-Al2O3 Catalysts Prepared from Layered Double Hydroxides" Catalysts 10, no. 5: 486. https://doi.org/10.3390/catal10050486

APA Style

R. Bertolini, G., Jiménez-Gómez, C. P., Cecilia, J. A., & Maireles-Torres, P. (2020). Gas-Phase Hydrogenation of Furfural to Furfuryl Alcohol over Cu-ZnO-Al2O3 Catalysts Prepared from Layered Double Hydroxides. Catalysts, 10(5), 486. https://doi.org/10.3390/catal10050486

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.