Next Article in Journal
Artificial Neural Network Modeling of Glass Transition Temperatures for Some Homopolymers with Saturated Carbon Chain Backbone
Next Article in Special Issue
Polymer Composite Fabrication Reinforced with Bamboo Fiber for Particle Board Product Raw Material Application
Previous Article in Journal
A Mini-Review on Recent Developments in Anti-Icing Methods
Previous Article in Special Issue
Prolonged Thermal Relaxation of the Thermosetting Polymers
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Kinetic Assessment of Mechanical Properties of a Cellulose Board Aged in Mineral Oil and Synthetic Ester

by
Cristina Fernández-Diego
1,*,
Alfredo Ortiz
1,
Isidro A. Carrascal
2,
Inmaculada Fernández
1 and
Carlos J. Renedo
1
1
Electrical and Energy Engineering Department, School of Industrial and Telecomunications Engineering, University of Cantabria, Avenida Los Castros, 39005 Santander, Cantabria, Spain
2
LADICIM (Laboratory of Materials Science and Engineering), School of Civil Engineering, University of Cantabria, Avenida Los Castros 44, 39005 Santander, Cantabria, Spain
*
Author to whom correspondence should be addressed.
Polymers 2021, 13(23), 4150; https://doi.org/10.3390/polym13234150
Submission received: 22 October 2021 / Revised: 21 November 2021 / Accepted: 22 November 2021 / Published: 27 November 2021
(This article belongs to the Special Issue Advances in the Mechanical Behavior of Polymeric Materials)

Abstract

:
In oil-immersed power transformers, the insulation system is constituted of a dielectric oil–solid combination. The insulation oil generally used is mineral oil; however, this fluid has started to be substituted by natural and synthetic esters due to their higher biodegradability and flash point. The introduction of a new fluid in the insulation system of power transformers requires kinetic models that can estimate the degradation rate of insulation solids. The aim of this work was to go further in quantifying through different kinetic models the deterioration suffered by a commercial cellulose board (PSP 3055), which is one of the solid materials used in the insulation system of oil-filled transformers. The aging study was extended to cellulose board specimens immersed in two different oils (mineral and synthetic ester). It was obtained that there is a lower degradation when synthetic ester is used in the insulation system. Additionally, it can be concluded that the use of mechanical properties to quantify the degradation of the cellulose board through kinetic models provides information about the different behavior shown by PSP 3055 when different fiber direction angles are considered.

1. Introduction

Transformers are critical machines to ensure power systems run properly [1]. In oil-immersed transformers, cellulose solids play a critical role as insulating materials [2], and they are impregnated with insulating oil to resist electric current between conductors. Moreover, the oil is used as a cooling means to evacuate high temperature while transformers are working [3].
During transformers’ operation, the insulation solid degrades slowly to its disintegration [4]. Although the oil also suffers aging, it can be regenerated or replaced easily; therefore, the life of a transformer is determined by its insulation solid.
Due to its high-coolant capability and its excellent dielectric behavior, mineral oil has been used widely as an insulating medium in oil-immersed transformers. Nonetheless, this liquid has impacted the environment because of its non-biodegradability. Moreover, mineral oil possesses poor fire-resistant characteristics, which have encouraged the search for biodegradable choices such as natural and synthetic esters [5,6].
There are works in which the aging characteristics of insulation systems based on esters have been described by focusing on the degradation of fluids [7,8,9] or of solids [10,11,12,13].
Pressboard is a cellulose-based insulation utilized as insulating material for making a variety of components in the design of transformers. This component experiences progressive loss of its mechanical strength, reducing its short-circuit withstand capability [14]. For this reason, the establishment of kinetic models can be an extremely useful tool to estimate the remaining life of insulation solids [15], making it possible to estimate the most suitable moment to replace power transformers [16].
Several works have evaluated the remaining life of insulating solids immersed in different insulation liquids using a wide range of measurements [1,5,15,17,18] in laboratory aging tests. Additionally, the through-thickness compression behavior of mineral oil-impregnated cellulose board [14], the chemical composition and surface topography of impregnated cellulose board samples [19,20], and the change in crystallographic parameters through dilatometry and X-ray diffraction analysis [2] have been studied. All these works in which esters have been considered have concluded that biodegradable dielectric liquids can prolong the life span of cellulose compared with mineral oil.
Although there are studies that have deal with cellulose-board degradation, there are no works in which a detailed kinetic assessment of cellulose-board aged in synthetic ester and mineral oil has been presented. This study aimed at a better understanding of the aging of cellulose-board in synthetic oil-filled transformers. Aging of solid insulation in synthetic ester was also compared with that in mineral oil. Deterioration status of cellulose-board is determined using the degree of polymerization (DP) and mechanical properties such as tensile strength and strain. These mechanical properties can be used as an approximate approach to explain how cellulose board breaks. The application of different kinetic models for characterizing the aging of cellulose-board was extensively studied to determine which one might be the most suitable. Additionally, the kinetic parameters of insulation cellulose-board PSP 3055 aged in mineral and synthetic ester were determined to define the effect of insulation liquid on the degradation rate for the cellulose-board.

2. Kinetic Modelling

Synthetic esters are obtained through an esterification reaction using polyols and saturated fatty acid groups [21]. Their different molecular structure in comparison with mineral oil determines their distinct physicochemical properties. One of them has higher moisture solubility in synthetic esters in comparison with mineral oil, which is beneficial because it attracts more moisture from cellulose insulation, increasing the life of the solid insulation. Hydrolysis, which is a decisive chemical reaction involved with water and oil structure, is also critical. The moisture dissolved in the insulation liquid reacts with ester, generating long chain fatty acids, which prevent moisture from moving into the cellulose solid [22].
In this study, different kinetic models (Table 1) were considered to quantify the deterioration suffered by cellulose-board during thermal aging in mineral and synthetic ester. These models were applied using the DP, tensile strength, and strain. The aim was to determine which one is the most suitable to simulate the deterioration of the insulation solid analyzed in this article (PSP 3055).

3. Materials and Methods

3.1. Material

The insulation systems for this work are composed of insulation oil and a cellulose-board (PSP 3055), whose properties are gathered in Table 2. A high-performance mineral oil and an environment-friendly synthetic ester were used as insulation liquids. Table 3 gives the essential characteristics of both liquids (a naphthenic oil and a synthetic ester).

3.2. Thermal Aging

The accelerated tests carried out in the laboratory were fast procedures to simulate the deterioration process quickly, and they can be used to estimate the remaining life under normal operation of the power transformer.
Although there are different properties that impact cellulose aging, in this work we only considered the effect of temperature because as it was demonstrated by Vasovic [29] that temperature has a stronger impact on aging than water content in insulation paper.
To carry out the accelerated thermal aging tests, the cellulose-board was cut into strips of 260 mm × 15 mm. Due to cellulose-board anisotropy, these strips were cut with two different fiber direction angles (machine (MD) and cross direction (CD)).
Secondly, the cellulose-board strips were dried under vacuum at 100 °C for 24 h, then placed them into stainless steel vessels, which were closed and sited in an oven, providing samples with a moisture content of around 2%.
Once the cellulose-board samples were dried, they were placed in oil in stainless steel vessels, which were sealed with nitrogen, and accelerated thermal aging tests were carried out. Aging vessels were placed in an air-circulating oven (UN110, Memmert, Schwabach, Germany) for thermal stressing at different temperatures and duration tests. The aging conditions were 150 °C for 953 h, 130 °C for 2263 h, and 110 °C for 16,155 h of thermal aging. During the aging periods, different samples of cellulose-board were taken out for testing (10 strips for each fiber direction angles). A vessel for each temperature and each oil was prepared by inserting 750 mL of new oil (mineral and synthetic ester) with a nitrogen headspace of 25% by volume.

3.3. Characterization

The degree of polymerization (DP) is recognized as an objective detection method to measure the rate of degradation of cellulose products used in transformers’ insulation systems [1,18]. Consequently, in this study, the DP of each group of specimens of PSP 3055 was measured following the viscometric method of the standard ASTM D4243.
The tensile test is also recognized as an objective detection method to evaluate the mechanical strength of cellulose-board when a specimen is clamped in an axial loading frame. The data obtained from this test (load and displacement) were used to determine tensile strength (σR) and strain under ultimate strength (εcm) because they are two parameters that provide suitable information about the real deterioration suffered by the insulation solid [12].
In this work, a universal servo hydraulic test machine (Model ME-405-1, SERVOSIS, Madrid, Spain) was used to carry out the tensile tests according to ISO 1924-2.

4. Results and Discussion

This section shows the degradation suffered by cellulose-board aged in mineral and synthetic ester.

4.1. DP and Mechanical Properties during Thermal Aging

Figure 1, Figure 2, Figure 3, Figure 4 and Figure 5 show DP, tensile strength (σR), and strain (εcm) curves for cellulose-board artificially aged at three different temperatures. Bulleted lists look like this:
The results showed that the damage increased over time and this increase became faster with the rise of temperature in both insulation liquids (mineral oil and synthetic ester). At the three temperatures, it was observed that the synthetic ester preserved better the state of the cellulose-board for the same aging time. The deterioration suffered by PSP, as was explained previously, is suggested to be distinct due to the different moisture equilibriums between oil and paper and hydrolysis reactions. However, this protective effect of synthetic ester seemed to be less significant as the temperature was reduced. The reason for that is unclear, but it might be associated with the water generated as a by-product of the deterioration, which played a more critical role in the degradation of the cellulose at higher temperatures, raising the rate of bond scission [30]. Since, in insulation systems based on synthetic ester/solid, the moisture tends to remain in the oil, obtaining an insulation solid drier, the effect of synthetic ester is more beneficial when the temperature is higher.
In the case of the mechanical properties considered in this work (σR and εcm), the observed behavior was similar to that found for DP. However, when these kinds of properties are evaluated, their values depend on the orientation of the paper’s fibers with respect to the applied load during the tensile test due to cellulose-board’s anisotropy. The values of σR, when the PSP fibers are in the same direction as that with which the test machine applies the load (MD), have been found to be two times the ones measured when the fibers are in a cross direction (CD) to the test machine, while the εcm is half approximately. This different behavior must be taken into consideration since, depending on the way the material is placed and the voltages are applied during the transformer operation, the cellulose-board resistance can be considerably affected. When a load is applied with fibers aligned, the fibers length is higher, and this contributes to an increase in the mechanical strength of the insulation solid.
For all the properties (DP, σR, and εcm), it was found that there was an important linear decrease at the beginning of thermal aging and a later stabilization of the values. Additionally, the loss of mechanical properties was observed in a similar way when fiber orientation was MD and CD.
Once the experimental values of the DP, σR, εcm, and the uncertainties were obtained, the correlation between these experimental data and the adjustment performed according to different kinetic models was analyzed. Additionally, the propagation of uncertainties in kinetic parameters and the coefficient of determination are summarized in the following section.

4.2. Ekenstam Kinetic Model

Ekenstam defined a kinetic model based on first-order chemical kinetic considerations (Table 1). The graph of (1/εcm − 1/εcm0) against time using experimental data and the model proposed by Ekenstam are plotted in Figure 6 for PSP 3055 at three different temperatures.
Similar representations were carried out for (1/DP − 1/DP0) and (1/σR − 1/σR0). These graphs were used to determine the constant rate of reaction for each temperature and insulation liquid, and their values are gathered in Table 4.
Although the values of the coefficients of determination (R2), which were obtained, were high enough for some aging conditions in mineral oil, they reveal there was not a suitable agreement between experimental values (DP, σR, and εcm) and the Ekenstam model when the cellulose-board was aged in synthetic ester.
It was verified that the constant rates of reaction increased considerably with the aging temperature. When the constant rates of mineral oil were compared with those calculated for synthetic ester, it was verified that these constants were higher. Therefore, the insulation liquid impacted the solid degradation substantially.

4.3. Emsley Kinetic Model

The equation proposed by Ekenstam was modified by Emsley et al. [24] because they observed that, whether the DP value of insulation paper decreases to a certain value, its behavior gradually deviates from the first-order kinetic (Table 1).
The change in rate constant seemed to be related with the inhomogeneous composition of the cellulosic solid (cellulose, lignin, and hemicelluloses). Additionally, it is known that the amorphous regions of cellulose are more reactive than the crystalline regions in which the degradation is very slow due to the higher order in cellulose chains, which reduces the accessibility of aging agents [31].
The constants of the Emsley et al. model [24] were obtained through the representation of (1/σR − 1/σR0), (1/εcm − 1/εcm0), and (1/DP − 1/DP0) against time for PSP 3055 at the aging temperatures and the studied insulation liquids. In Figure 7 is shown the shape of the curves of Emsley’s model based on tensile strength. Similar representations were obtained for εcm and DP.
The values of both constants (k10 and k2) are gathered in Table 5. This kinetic model had a high agreement with the experimental measures, with all the coefficients of determination (R2) being higher than 0.84. The three properties considered in this study seemed to be suitable to estimate PSP 3055 deterioration using this kinetic model.
As previously, it was verified that the constants of this kinetic model were highly influenced by the aging temperature and type of oil.

4.4. Zervos’ Kinetic Model

Although this model was defined from the study of pure cotton cellulose, it was used to model the deterioration of cellulose-board measured in this work.
The constants of the Zervos model [25] were obtained through the representation of (1/σR – 1/σR0), (1/εcm – 1/εcm0), and (1/DP – 1/DP0) against time, as with previous models. The curves obtained from the measures of the DP of the pressboard are shown in Figure 8. This representation was also done for εcm and σR.
The values of the calculated constants (k and a) are shown in Table 6. This kinetic model had a high agreement with the experimental measures, with the coefficients of determination (R2) being slightly lower than the ones obtained with the Emsley model.
Both mechanical properties (εcm and σR) and the DP allowed us to estimate the degradation of the PSP 3055 through this mathematical approach.

4.5. Calvini Kinetic Model

The kinetic models used in previous sections only dealt with the extent of cellulose degradation in terms of the ratio of broken glucose units to the total glucose units of a cellulose chain (SFCU = 1/DP − 1/DP0). As was pointed out by Calvini and Gorassini [26], every experimental uncertainty about the actual values of DP0 and DP is amplified in the determination of the cellulosic solids’ degradation. For this reason, those authors introduced the concept of S = (DP0/DP) − 1, which represents the average number of chain scissions per cellulose chain unit during the time of degradation. Additionally, they considered the so-called levelling-off value (LODP), which means the beginning of a third, very slow degradation stage of the cellulose. This stage can be found only with very drastic degradations, in a range of DP below the so-called levelling-off value, where nothing but crystallites remain and the tensile strength of cellulose is lost forever. Before this third stage, there are two distinct stages: a fast initial attack to the so-called weak links followed by a slower one to the amorphous fraction.
To apply this model, in this work we established for LODP a DP of 200, εcm, and σR (25% of initial value) [32].
The constant of the Calvini and Gorassini model [26] was obtained through the representation of (σR0R − 1), (εcm0cm − 1), and (DP0/DP − 1) against time. The curves based on strain are gathered in Figure 9. The same representation was carried out for σR and DP.
The values of the constant rate of reaction (k) are gathered in Table 7. It can be observed that there was not a suitable agreement between experimental values (DP, σR, and εcm) and the Calvini mathematical approach.
On the other hand, it was found that the values of DP, σR, and εcm selected as levelling off possessed a huge impact on the R2. Moreover, this impact depended on the aging temperature, insulation liquid, and property used to quantify the deterioration suffered by PSP 3055. Therefore, this mathematical approach seemed to be influenced by different variables, which makes its application more complicated in comparison with other models.

4.6. Weidmann Kinetic Model

This was one of the earliest models formulated empirically by researchers at Weidmann [27].
The representation of ln(σRR0), ln (εcmcm0), and ln (DP/DP0) against time allowed us to obtain the values of the coefficient of aging of this model [27]. Figure 10 displays the curves based on tensile strength. The curves based on strain and DP were also done.
The values of the coefficient of aging are shown in Table 8. The coefficients of determination (R2) were low; in consequence, the Weidmann model did not allow us to make a good estimation of the cellulose-board deterioration.

4.7. IEEE Kinetic Model

The constants of this mathematical approach were calculated using the representation of ln (time required to reach the end-of-life criteria) versus inverse temperature (1/T), resulting in a linear curve, as can be seen in the Figure 11. To guarantee that the end-of-life criteria was reached for all the conditions studied in this article, the following aging stages were established as points of comparison: DP = 350, σR = 0.50 ∗ σR0, and εcm = 0.50 ∗ εcm0.
The values of the constants of the IEEE mathematical approach are displayed in Table 9. Although the calculated coefficients of determination (R2) were high, they reduced their values when the insulation solid underwent a greater deterioration, which happened when the samples of PSP 3055 were aged in mineral oil. On the other hand, it was necessary to highlight the effect that the criterion established as end of life had on the results. In this work, the values of DP, σR, and εcm established as points of comparison were quite high, being located approximately in the fast-initial attack to the insulation solid during thermal aging. Therefore, it would be convenient to carry out longer aging tests at low temperatures to apply end-of-life criteria in which the material would have experienced higher deterioration, obtaining more information about the suitability of this model.

5. Conclusions

Different kinetic models based on the variation of degree of polymerization (DP), tensile strength (σR), and strain (εcm) were used to quantify the deterioration of cellulose-board PSP 3055 aged in mineral oil and synthetic ester.
The measurement of DP and the mechanical properties (σR and εcm) showed the effect of the insulation liquid on the degradation suffered by cellulose-board during thermal aging, concluding there was a lower degradation when synthetic ester was used in the insulation system.
It was been obtained that the kinetic models proposed by Emsley [24] and Zervos [25] allowed us to obtain the highest correlation coefficients in both mineral and synthetic ester. Moreover, it was found that the suitability and accuracy of some of the models applied in this work [26,28] depended on the levelling-off value established for the constant rate calculation or the end-of-life criteria established as a point of comparison, which made their implementation more challenging and complex.
In all the kinetic models considered in this paper, their characteristic parameters, as well as their correlation coefficients, suffered variations in their values that were generally lower than 10% when the uncertainties in measurements were considered, which validated the robustness of the observed trends during thermal aging in both insulation liquids.
Additionally, it can be concluded that the use of mechanical properties to quantify the degradation of the cellulose-board evaluated in this study through a kinetic model provided information about the different behavior shown by PSP 3055 when different fiber direction angles (MD and CD) were considered. Therefore, kinetic models based on mechanical properties make possible the assessment of the effect of cellulose-board anisotropy, which cannot be considered when DP is used to evaluate its aging.

Author Contributions

Conceptualization, C.F.-D., A.O., I.A.C., I.F. and C.J.R.; methodology, C.F.-D., A.O., I.A.C., I.F. and C.J.R.; validation, C.F.-D., A.O., I.A.C., I.F. and C.J.R.; formal analysis, C.F.-D., A.O., I.A.C., I.F. and C.J.R.; investigation, C.F.-D., A.O., I.A.C., I.F. and C.J.R.; resources, C.F.-D., A.O., I.A.C., I.F. and C.J.R.; data curation, C.F.-D., A.O., I.A.C., I.F. and C.J.R.; writing—original draft preparation, C.F.-D., A.O., I.A.C., I.F. and C.J.R.; writing—review and editing, C.F.-D., A.O., I.A.C., I.F. and C.J.R. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by State Scientific and Technical Research and Innovation Plan under the PID2019-107126RB-C22/AEI/10.13039/501100011033 grant agreement, financed by the Government of Spain.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Data is contained within the article.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Saldivar-Guerrero, R.; Cabrera Álvarez, E.N.; Leon-Silva, U.; Lopez-Gonzalez, F.A.; Delgado Arroyo, F.; Lara-Covarrubias, H.; Montes-Fernandez, R. Quantitative Analysis of Ageing Condition of Insulating Paper Using Infrared Spectroscopy. Adv. Mater. Sci. Eng. 2016, 2016, 6371540. [Google Scholar] [CrossRef] [Green Version]
  2. Mohan Rao, U.; Jarial, R.K. Measurement of transformer solid insulation degradation using dilatometry and X-ray diffraction analysis. Meas. J. Int. Meas. Confed. 2019, 131, 701–705. [Google Scholar] [CrossRef]
  3. Santisteban, A.; Piquero, A.; Ortiz, F.; Delgado, F.; Ortiz, A. Thermal Modelling of a Power Transformer Disc Type Winding Immersed in Mineral and Ester-Based Oils Using Network Models and CFD. IEEE Access 2019, 7, 174651–174661. [Google Scholar] [CrossRef]
  4. Łojewski, T.; Miśkowiec, P.; Missori, M.; Lubańska, A.; Proniewicz, L.M.; Łojewska, J. FTIR and UV/vis as methods for evaluation of oxidative degradation of model paper: DFT approach for carbonyl vibrations. Carbohydr. Polym. 2010, 82, 370–375. [Google Scholar] [CrossRef]
  5. Li, S.; Zhao, X.; Liao, R.; Yang, L.; Guo, P. Study on ageing characteristics of insulating pressboard impregnated by mineral-vegetable oil. In Proceedings of the 2016 IEEE Conference on Electrical Insulation and Dielectric Phenomena (CEIDP), Toronto, ON, Canada, 16–19 October 2016; pp. 70–73. [Google Scholar] [CrossRef]
  6. Rozga, P.; Beroual, A.; Przybylek, P.; Jaroszewski, M.; Strzelecki, K. A Review on Synthetic Ester Liquids for Transformer Applications. Energies 2020, 13, 6429. [Google Scholar] [CrossRef]
  7. Mahidhar, G.D.P.; Karthikeyan, A.S.; Sarathi, R.; Taylor, N.; Edin, H. Dielectric properties of mixed mineral and synthetic ester oil. IET Sci. Meas. Technol. 2020, 14, 704–714. [Google Scholar] [CrossRef]
  8. Martins, M.A.G.; Gomes, A.R. Comparative study of the thermal degradation of synthetic and natural esters and mineral oil: Effect of oil type in the thermal degradation of insulating kraft paper. IEEE Electron. Insul. Mag. 2012, 28, 22–28. [Google Scholar] [CrossRef]
  9. Vihacencu, M.Ş.; Ciuriuc, A.; Dumitran, L.M. Experimental study of electrical properties of mineral and vegetable transformer oils. UPB Sci. Bull. Ser. C Electron. Eng. 2013, 75, 171–182. [Google Scholar]
  10. Carcedo, J.; Fernandez, I.; Ortiz, A.; Delgado, F.; Renedo, C.J.; Arroyo, A. Quantitative study on the aging of kraft paper in vegetable oils. IEEE Electron. Insul. Mag. 2016, 32, 29–35. [Google Scholar] [CrossRef]
  11. García, B.; García, T.; Primo, V.; Burgos, J.C.; Urquiza, D. Studying the loss of life of natural-ester-filled transformer insulation: Impact of moisture on the aging rate of paper. IEEE Electron. Insul. Mag. 2017, 33, 15–23. [Google Scholar] [CrossRef]
  12. Carrascal, I.A.; Fernández-Diego, C.; Casado, J.A.; Diego, S.; Fernández, I.; Ortiz, A. Quantification of Kraft paper ageing in mineral oil impregnated insulation systems through mechanical characterization. Cellulose 2018, 25, 3583–3594. [Google Scholar] [CrossRef] [Green Version]
  13. Fernandez, O.H.A.; Fofana, I.; Jalbert, J.; Gagnon, S.; Rodriguez-Celis, E.; Duchesne, S.; Ryadi, M. Aging characterization of electrical insulation papers impregnated with synthetic ester and mineral oil: Correlations between mechanical properties, depolymerization and some chemical markers. IEEE Trans. Dielectr. Electron. Insul. 2018, 25, 217–227. [Google Scholar] [CrossRef]
  14. Naranpanawe, L.; Ekanayake, C.; Saha, T.K. Measurements on pressboard to understand the effect of solid insulation condition on monitoring of power transformer winding clamping pressure. IET Sci. Meas. Technol. 2019, 13, 186–192. [Google Scholar] [CrossRef]
  15. Zhou, J.; Li, J.; Liao, R.; Lv, Y. Thermal aging properties of pressboard in mineral oil and natural ester. In Proceedings of the 2016 IEEE International Conference on High Voltage Engineering and Application (ICHVE), Chengdu, China, 19–22 September 2016. [Google Scholar] [CrossRef]
  16. Xie, F.; Bao, J.; Zhuo, L.; Zhao, Y.; Dang, W.; Si, L.; Yao, C.; Zhang, M.; Lu, Z. Toward high-performance nanofibrillated cellulose/aramid fibrid paper-based composites via polyethyleneimine-assisted decoration of silica nanoparticle onto aramid fibrid. Carbohydr. Polym. 2020, 245, 116610. [Google Scholar] [CrossRef] [PubMed]
  17. Suwarno Ritonga, A. Effects of thermal aging on the characteristics of kraft paper in various liquid insulating materials. In Proceedings of the 2020 International Symposium on Electrical Insulating Materials (ISEIM), Tokyo, Japan, 13–17 September 2020; pp. 15–24. [Google Scholar]
  18. Bandara, K.; Ekanayake, C.; Saha, T.K.; Annamalai, P.K. Understanding the ageing aspects of natural ester based insulation liquid in power transformer. IEEE Trans. Dielectr. Electron. Insul. 2016, 23, 246–257. [Google Scholar] [CrossRef]
  19. Li, Y.; Zhou, K.; Li, Z.R.; Zhang, Q.G. Research on the electrical aging characteristics of oil-impregnated pressboard under partial discharges. IEEE Trans. Dielectr. Electron. Insul. 2020, 27, 42–48. [Google Scholar] [CrossRef]
  20. Wang, Y.; Wang, Y.; Jiang, X. The microscopic morphology of insulation pressboard: An image processing perspective. Cellulose 2018, 25, 3051–3065. [Google Scholar] [CrossRef]
  21. Matic, E.; Meissner, M.; Schober, S.; Mittelbach, M. Volatile Acid and Polymer Formation in Various Insulation Liquids upon Accelerated Thermal Ageing. In Proceedings of the 2020 IEEE 3rd International Conference on Dielectrics (ICD), Valencia, Spain, 5–31 July 2020; pp. 720–723. [Google Scholar] [CrossRef]
  22. Rao, U.M.; Sood, Y.R.; Jarial, R.K.; Subrahmanyam, K. Preliminary studies on thermal ageing of alternate dielectric liquids for transformers. In Proceedings of the 2015 Annual IEEE India Conference (INDICON), New Delhi, India, 17–20 December 2015; pp. 1–5. [Google Scholar] [CrossRef]
  23. Ekenstam, A. The behaviour of cellulose in mineral acid solutions: Kinetic study of the decomposition of cellulose in acid solutions. BER 1936, 69, 553. [Google Scholar]
  24. Emsley, A.M.; Heywood, R.J.; Ali, M.; Eley, C.M. On the kinetics of degradation of cellulose. Cellulose 1997, 4, 1–5. [Google Scholar] [CrossRef]
  25. Zervos, S.; Moropoulou, A. Cotton cellulose ageing in sealed vessels. Kinetic model of autocatalytic depolymerization. Cellulose 2005, 12, 485–496. [Google Scholar] [CrossRef]
  26. Calvini, P.; Gorassini, A. On the rate of paper degradation: Lessons from the past. Restaurator 2006, 27, 275–290. [Google Scholar] [CrossRef]
  27. Gasser, H.P.; Huser, J.; Krause, C.; Dahinden, V.; Emsley, A.M. Determining the ageing parameters of cellulosic insulation in a transformer. IEE Conf. Publ. 1999, 4, 1–5. [Google Scholar] [CrossRef]
  28. IEEE. C57.91 Guide for Loading Mineral-Oil-Immersed Transformers and Step-Voltage Regulators; IEEE: Geneva, Switzerland, 2011. [Google Scholar]
  29. Vasovic, V.; Lukic, J.; Mihajlovic, D.; Pejovic, B.; Milovanovic, M.; Radoman, U.; Radakovic, Z. Aging of transformer insulation of experimental transformers and laboratory models with different moisture contents: Part II—Moisture distribution and aging kinetics. IEEE Trans. Dielectr. Electron. Insul. 2019, 26, 1847–1852. [Google Scholar] [CrossRef]
  30. Hill, D.J.T.; Le, T.T.; Darveniza, M.; Saha, T. A study of degradation of cellulosic insulation materials in a power transformer, part 1. Molecular weight study of cellulose insulation paper. Polym. Degrad. Stab. 1995, 48, 79–87. [Google Scholar] [CrossRef]
  31. Lukic, J.; Deville, K.; Lessard, M.C.; Dreier, L.; Hohlein, I.A.; Vrsaljko, D.; Peixoto, A.; Melzer, L.; Leward, L.; Ding, H. Changes of new unused insulating kraft paper properties during drying—Impact on degree of polymerization. Cigrè Sci. Enginnering 2021, 20, 161–170. [Google Scholar]
  32. IEC 60076-7 Power Transformers—Part 7: Loading Guide for Mineral-Oil-Immersed Power Transformers; IEC: Geneva, Switzerland, 2018.
Figure 1. Evolution of the DP as a function of temperature for cellulose-board PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c).
Figure 1. Evolution of the DP as a function of temperature for cellulose-board PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c).
Polymers 13 04150 g001
Figure 2. Evolution of the σR in MD as a function of temperature for cellulose-board PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c).
Figure 2. Evolution of the σR in MD as a function of temperature for cellulose-board PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c).
Polymers 13 04150 g002
Figure 3. Evolution of the σR in CD as a function of temperature for cellulose-board PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c).
Figure 3. Evolution of the σR in CD as a function of temperature for cellulose-board PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c).
Polymers 13 04150 g003aPolymers 13 04150 g003b
Figure 4. Evolution of the εcm in MD as a function of temperature for cellulose-board PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c).
Figure 4. Evolution of the εcm in MD as a function of temperature for cellulose-board PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c).
Polymers 13 04150 g004
Figure 5. Evolution of the εcm in CD as a function of temperature for cellulose-board PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c).
Figure 5. Evolution of the εcm in CD as a function of temperature for cellulose-board PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c).
Polymers 13 04150 g005
Figure 6. Evolution of the (1/εcm − 1/εcm0) in MD and CD as a function of temperature for pressboard PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c) and Ekenstam’s function.
Figure 6. Evolution of the (1/εcm − 1/εcm0) in MD and CD as a function of temperature for pressboard PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c) and Ekenstam’s function.
Polymers 13 04150 g006
Figure 7. Evolution of the (1/εcm − 1/εcm0) in MD and CD as a function of temperature for pressboard PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c) and Emsley’s function.
Figure 7. Evolution of the (1/εcm − 1/εcm0) in MD and CD as a function of temperature for pressboard PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c) and Emsley’s function.
Polymers 13 04150 g007
Figure 8. Evolution of the (1/DP -1/DP0) as a function of temperature for pressboard PSP 3055 aged at 150 °C, 130 °C, and 110 °C, and Zervos’ function, in mineral oil (a) and in synthetic ester (b).
Figure 8. Evolution of the (1/DP -1/DP0) as a function of temperature for pressboard PSP 3055 aged at 150 °C, 130 °C, and 110 °C, and Zervos’ function, in mineral oil (a) and in synthetic ester (b).
Polymers 13 04150 g008
Figure 9. Evolution of the (εcm0cm) − 1 in MD and CD as a function of temperature for pressboard PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c) and Calvini’s function.
Figure 9. Evolution of the (εcm0cm) − 1 in MD and CD as a function of temperature for pressboard PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c) and Calvini’s function.
Polymers 13 04150 g009
Figure 10. Evolution of the ln (σRR0) in MD and CD as a function of temperature for pressboard PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c) and Weidmann’s function.
Figure 10. Evolution of the ln (σRR0) in MD and CD as a function of temperature for pressboard PSP 3055 aged in mineral oil and in synthetic ester at 150 °C (a), 130 °C (b), and 110 °C (c) and Weidmann’s function.
Polymers 13 04150 g010
Figure 11. Evolution of the ln (time) vs. inverse temperature in CD for pressboard PSP 3055 aged in mineral oil considering: εcm (a), σR (b), and DP (c).
Figure 11. Evolution of the ln (time) vs. inverse temperature in CD for pressboard PSP 3055 aged in mineral oil considering: εcm (a), σR (b), and DP (c).
Polymers 13 04150 g011
Table 1. Kinetic models of cellulose solid deterioration.
Table 1. Kinetic models of cellulose solid deterioration.
Ekenstam Kinetic model
( 1 / D P ) ( 1 / D P 0 ) = k t (1)[23]
where D P 0 is the Number of average degree of polymerization at the time of 0, D P is the Number of average degree of polymerization at the time of t, k is the Constant rate of reaction, and t is the Aging time (h).
Emsley kinetic model
( 1 / D P ) ( 1 / D P 0 ) = ( k 1 0 / k 2 ) 1 e x p k 2 t (2)[24]
where K 1 0 and K 2 are Temperature-dependent constants.
Zervos Kinetic model
( 1 / D P ) ( 1 / D P 0 ) = ( a / 100 ) 2 k t 1 (3)[25]
where k and a are Temperature-dependent constants.
Calvini Kinetic model
( D P 0 / D P ) 1 = ( D P 0 / L O D P ) 1 e x p k t (4)[26]
where L O D P is the Leveling-off degree of polymerization.
Weidmann Kinetic model
T S = T S 0 e x p C T S T t (5)[27]
D P = D P 0 e x p C D P T t (6)
where T S is the Tensile strength aged, T S 0 is the Tensile strength unaged and C T S and C D P are Coefficients of aging.
IEEE Kinetic model
ln L T = A + B / T o r L T = A e x p B / T (7)[28]
where ln L T is the Lifetime of the power transformer and A and B are Temperature-dependent constants.
Table 2. PSP 3055 properties.
Table 2. PSP 3055 properties.
PropertyValue
Apparent density (kg/m3)1100 ± 6.20%
Degree of polymerization (before impregnation)750 ± 9.50%
pH of aqueous extract7.20 ± 8.41%
Moisture content (%)<8 ± 4.32%
Ash content (%)0.30 ± 8.22%
Conductivity of aqueous extract (mS/m)2.0 ± 9.70%
Electric strength in air unfolded (kV/mm)7 ± 3.11%
Electric strength in oil (kV/mm)50 ± 5.40%
Table 3. Properties of commercial oils analyzed.
Table 3. Properties of commercial oils analyzed.
PropertyStandardMineral Oil (MO)Synthetic Ester (SE)
Viscosity, 40 °C (mm2/s)ISO 3104, ASTM D44510.30 ± 2.90%29 ± 12.70%
Density, 20 °C (kg/dm3)ISO 3675, ASTM D40520.84 ± 6.50%0.97 ± 3.20%
Pour point (°C)ISO 3016, ASTM D97−63 ± 9.70%−56 ± 10.00%
Flash point (°C)ISO 2719, ASTM D92160 ± 8.60%260 ± 9.20%
Water content (mg/kg)IEC 6081415 ± 8.70%50 ± 11.50%
Breakdown voltage (kV)IEC 60156>70 ± 7.30%>75 ± 12.40%
Acidity (mg KOH/g)IEC 62021.1, ASTM D974<0.01 ± 1.70%<0.03 ± 3.20%
Dielectric dissipation factor (90 °C)IEC 602477 × 10−4 ± 8.20%<8 × 10−3 ± 12.80%
Table 4. Constant rates of reaction for Ekenstam model based on DP, εcm, and σR for different insulation oils.
Table 4. Constant rates of reaction for Ekenstam model based on DP, εcm, and σR for different insulation oils.
( 1 / P r o p e r t y   D P ,   ε c m ,   σ R ( 1 / P r o p e r t y   0   D P ,   ε c m ,   σ R ) = k × t
Mineral oil Synthetic ester
Temperature (°C)k (DP)R2k (DP)R2
1501.30 × 10−5 ± 10.47%0.74 ± 0.82%3.72 × 10−6 ± 11.29%0.72 ± 9.33%
1304.41 × 10−6 ± 11.96%0.80 ± 0.06%1.01 × 10−6 ± 12.07%0.49 ± 4.84%
1101.65 × 10−7 ± 8.76%0.86 ± 0.55%1.17 × 10−7 ± 8.26%0.07 ± 12.38%
Temperature (°C)k (εcm) CDR2k (εcm) CDR2
1504.48 × 10−1 ± 6.31%0.89 ± 0.47%1.01 × 10−1 ± 7.29%0.53 ± 8.03%
1301.67 × 10−1 ± 7.02%0.77 ± 2.28%1.15 × 10−2 ± 6.53%0.76 ± 4.86%
1101.32 × 10−3 ± 7.62%0.99 ± 4.22%6.73 × 10−4 ± 3.89%0.77 ± 9.04%
Temperature (°C)k (εcm) MDR2k (εcm) MDR2
1506.67 × 10−1 ± 6.83%0.87 ± 0.34%3.84 × 10−1 ± 4.69%0.81 ± 2.70%
1303.46 × 10−1 ± 5.87%0.79 ± 1.01%3.13 × 10−2 ± 8.99%0.63 ± 3.56%
1103.05 × 10−3 ± 9.08%0.66 ± 11.07%1.70 × 10−3 ± 11.76%0.03 ± 7.65%
Temperature (°C)k (σR) CDR2k (σR) CDR2
1502.06 × 10−7 ± 5.13%0.94 ± 1.25%5.55 × 10−8 ± 6.50%0.37 ± 1.94%
1309.49 × 10−8 ± 11.82%0.77 ± 0.06%1.16 × 10−8 ± 5.54%0.54 ± 5.43%
1101.46 × 10−9 ± 8.74%0.83 ± 6.12%1.30 × 10−9 ± 9.16%0.45 ± 6.10%
Temperature (°C)k (σR) MDR2k (σR) MDR2
1501.54 × 10−7 ± 3.89%0.83 ± 3.32%6.79 × 10−8 ± 4.62%0.83 ± 0.82%
1306.58 × 10−8 ± 7.86%0.75 ± 2.58%5.94 × 10−9 ± 9.22%0.74 ± 7.06%
1108.13 × 10−10 ± 11.28%0.93 ± 0.48%6.12 × 10−6 ± 9.98%0.81 ± 1.43%
Table 5. Constant rates of reaction for the Emsley model based on DP, εcm, and σR for different insulation oils.
Table 5. Constant rates of reaction for the Emsley model based on DP, εcm, and σR for different insulation oils.
( 1 / P r o p e r t y   D P ,   ε c m ,   σ R ( 1 / P r o p e r t y   0   D P ,   ε c m ,   σ R ) = ( k 1 0 / k 2 ) × 1 e x p k 2 × t
Mineral oil Synthetic ester
Temperature (°C)k10 (DP)k2 (DP)R2k10 (DP)k2 (DP)R2
1503.23 × 10−5 ± 9.31%3.02 × 10−3 ± 1.23%0.99 ± 0.40%9.59 × 10−6 ± 0.78%3.18 × 10−3 ± 8.30%0.98 ± 0.19%
1309.97 × 10−6 ± 10.35%1.12 × 10−3 ± 0.97%0.96 ± 0.52%3.85 × 10−6 ± 9.80%2.28 × 10−3 ± 3.46%0.96 ± 1.82%
1103.43 × 10−7 ± 8.26%1.25 × 10−4 ± 0.94%0.97 ± 0.51%5.03 × 10−7 ± 10.20%3.36 × 10−4 ± 9.96%0.91 ± 4.66%
Temperature (°C)k10cm) CDk2cm) CDR2k10cm) CDk2cm) CDR2
1502.89 × 10−1 ± 10.54%−1.05 × 10−3 ± 9.69%0.92 ± 0.13%3.59 × 10−1 ± 0.66%4.84 × 10−3 ± 8.61%0.98 ± 1.16%
1303.95 × 10−1 ± 4.22%1.20 × 10−3 ± 4.46%0.97 ± 0.24%2.79 × 10−2 ± 10.93%1.25 × 10−3 ± 8.46%0.97 ± 0.61%
1101.49 × 10−3 ± 6.23%1.66 × 10−5 ± 9.54%0.99 ± 1.30%1.74 × 10−3 ± 10.85%1.72 × 10−4 ± 10.16%0.96 ± 1.91%
Temperature (°C)k10cm) MDk2cm) MDR2k10cm) MDk2cm) MDR2
1508.27 × 10−1 ± 5.97%5.90 × 10−4 ± 4.49%0.87 ± 0.42%6.60 × 10−1 ± 8.20%1.61 × 10−3 ± 7.86%0.87 ± 3.89%
1308.03 × 10−1 ± 7.84%1.17 × 10−3 ± 3.25%0.96 ± 0.04%9.51 × 10−2 ± 9.56%1.69 × 10−3 ± 3.64%0.99 ± 0.08%
1108.94 × 10−3 ± 3.42%2.04 × 10−4 ± 7.71%0.94 ± 4.03%1.07 × 10−2 ± 7.80%5.43 × 10−4 ± 9.44%0.91 ± 2.72%
Temperature (°C)k10R) CDk2R) CDR2k10R) CDk2R) CDR2
1503.24 × 10−7 ± 10.19%1.31 × 10−3 ± 8.32%0.98 ± 0.11%2.47 × 10−7 ± 5.73%6.22 × 10−3 ± 0.99%0.99 ± 0.62%
1302.26 × 10−7 ± 9.60%1.21 × 10−3 ± 0.39%0.98 ± 0.23%4.07 × 10−8 ± 9.31%2.02 × 10−3 ± 4.43%0.95 ± 0.73%
1102.69 × 10−9 ± 8.53%9.98 × 10−5 ± 9.37%0.89 ± 7.73%5.17 × 10−9 ± 8.32%3.13 × 10−4 ± 7.24%0.91 ± 2.08%
Temperature (°C)k10R) MDk2R) MDR2k10R) MDk2R) MDR2
1502.66 × 10−7 ± 10.20%1.63 × 10−3 ± 5.20%0.90 ± 0.67%4.76 × 10−8 ± 8.84%−8.56 × 10−4 ± 10.11%0.85 ± 0.34%
1301.92 × 10−7 ± 8.20%1.26 × 10−3 ± 3.49%0.97 ± 0.05%1.54 × 10−8 ± 8.13%1.37 × 10−3 ± 8.82%0.99 ± 0.63%
1101.32 × 10−9 ± 8.16%7.63 × 10−5 ± 8.41%0.97 ± 1.59%1.07 × 10−9 ± 9.17%8.90 × 10−5 ± 9.62%0.87 ± 1.08%
Table 6. Constant rates of reaction for the Zervos model based on DP, εcm, and σR for different insulation oils.
Table 6. Constant rates of reaction for the Zervos model based on DP, εcm, and σR for different insulation oils.
( 1 / P r o p e r t y   D P ,   ε c m ,   σ R ( 1 / P r o p e r t y   0   D P ,   ε c m ,   σ R ) = ( a / 100 ) × 2 k × t 1
Mineral oilSynthetic ester
Temperature (°C)k (DP)a (DP)R2k (DP)a (DP)R2
150−4.35 × 10−3 ± 1.22%−1.07 ± 9.19%0.99 ± 0.40%−4.58 × 10−3 ± 9.39%−3.02 × 10−1 ± 10.78%0.98 ± 0.22%
130−1.62 × 10−3 ± 0.99%−8.89 × 10−1 ± 10.22%0.96 ± 0.55%−3.28 × 10−3 ± 3.35%−1.69 × 10−1 ± 9.66%0.96 ± 1.73%
110−1.80 × 10−4 ± 9.43%−2.75 × 10−1 ± 9.39%0.97 ± 0.51%−7.05 × 10−4 ± 10.63%−1.41 × 10−1 ± 7.22%0.94 ± 1.27%
Temperature (°C)k (εcm) CDa (εcm) CDR2k (εcm) CDa (εcm) CDR2
150−2.89 × 10−5 ± 8.66%−2.25 × 106 ± 10.10%0.89 ± 3.57%−7.04 × 10−3 ± 7.84%−7.39 × 103 ± 8.27%0.98 ± 1.08%
130−1.72 × 10−3 ± 4.46%−3.31 × 104 ± 8.31%0.97 ± 0.25%−1.80 × 10−3 ± 8.59%−2.24 × 103 ± 3.68%0.97 ± 0.60%
110−2.37 × 10−5 ± 9.16%−9.03 × 103 ± 10.76%0.99 ± 1.30%−2.49 × 10−4 ± 10.19%−1.01 × 103 ± 1.70%0.96 ± 1.90%
Temperature (°C)k (εcm) MDa (εcm) MDR2k (εcm) MDa (εcm) MDR2
150−8.47 × 10−4 ± 4.98%−1.41 × 105 ± 10.32%0.87 ± 0.41%−2.32 × 10−3 ± 7.87%−4.11 × 104 ± 0.73%0.87 ± 3.89%
130−1.69 × 10−3 ± 3.25%−6.88 × 104 ± 4.74%0.96 ± 0.49%−2.44 × 10−3 ± 3.67%−5.63 × 103 ± 8.19%0.99 ± 7.01%
110−2.94 × 10−4 ± 7.77%−4.38 × 103 ± 10.22%0.94 ± 4.05%−7.86 × 10−4 ± 4.06%−1.98 × 103 ± 10.62%0.91 ± 2.74%
Temperature (°C)k (σR) CDa (σR) CDR2k (σR) CDa (σR) CDR2
150−1.89 × 10−3 ± 11.22%−2.48 × 10−2 ± 3.52%0.99 ± 1.05%−9.21 × 10−3 ± 1.51%−3.98 × 10−3 ± 6.80%0.98 ± 3.70%
130−1.74 × 10−3 ± 5.01%−1.87 × 10−2 ± 11.96%0.98 ± 1.355%−2.91 × 10−3 ± 6.34%−2.02 × 10−3 ± 4.63%0.95 ± 1.73%
110−1.44 × 10−4 ± 7.81%−2.69 × 10−3 ± 5.14%0.89 ± 7.73%−4.52 × 10−4 ± 8.24%−1.65 × 10−3 ± 10.26%0.91 ± 2.07%
Temperature (°C)k (σR) MDa (σR) MDR2k (σR) MDa (σR) MDR2
150−2.35 × 10−3 ± 5.20%−1.63 × 10−2 ± 9.51%0.90 ± 0.89%−5.28 × 10−5 ± 8.69%−1.87 × 10−1 ± 10.74%0.83 ± 1.43%
130−1.82 × 10−3 ± 3.56%−1.28 × 10−2 ± 8.73%0.97 ± 1.04%−1.98 × 10−3 ± 9.37%−1.12 × 10−3 ± 5.03%0.99 ± 1.50%
110−1.10 × 10−4 ± 10.41%−1.73 × 10−3 ± 3.32%0.98 ± 1.57%−1.29 × 10−4 ± 9.77%−1.20 × 10−3 ± 2.24%0.87 ± 1.12%
Table 7. Constant rates of reaction for the Calvini model based on DP, εcm, and σR for different insulation oils.
Table 7. Constant rates of reaction for the Calvini model based on DP, εcm, and σR for different insulation oils.
( P r o p e r t y   0   D P ,   ε c m ,   σ R / P r o p e r t y   D P ,   ε c m ,   σ R ) 1 = ( P r o p e r t y   0 / L O P r o p e r t y ) × 1 e x p k × t
Mineral oil Synthetic ester
Temperature (°C)k (DP)R2k (DP)R2
1501.23 × 10−2 ± 3.64%0.25 ± 3.82%9.69 × 10−4 ± 0.54%0.88 ± 4.77%
1302.97 × 10−3 ± 1.65%0.75 ± 1.71%2.27 × 10−4 ± 1.43%0.62 ± 2.47%
1103.98 × 10−5 ± 3.85%0.92 ± 0.67%2.69 × 10−5 ± 3.03%0.21 ± 4.27%
Temperature (°C)k (εcm) CDR2k (εcm) CDR2
1505.10 × 10−1 ± 4.75%<0.01 ± 8.10%9.85 × 10−3 ± 2.15%0.78 ± 3.17%
1307.68 × 10−3 ± 3.25%<0.01 ± 4.20%2.61 × 10−4 ± 1.62%0.85 ± 3.24%
1102.83 × 10−5 ± 5.84%0.99 ± 1.05%1.33 × 10−5 ± 1.44%0.80 ± 8.22%
Temperature (°C)k (εcm) MDR2k (εcm) MDR2
1507.87 × 10−1 ± 3.98%<0.01 ± 1.12%7.41 × 10−1 ± 7.70%0.29 ± 4.98%
1308.63 × 10−3 ± 4.73%<0.01 ± 9.31%3.53 × 10−4 ± 6.39%0.80 ± 1.70%
1103.18 × 10−5 ± 5.06%0.75 ± 9.71%1.57 × 10−5 ± 8.33%0.11 ± 7.11%
Temperature (°C)k (σR) CDR2k (σR) CDR2
1509.61 × 10−1 ± 9.37%0.05 ± 6.41%4.75 × 10−3 ± 6.15%0.48 ± 9.56%
1303.38 × 10−3 ± 5.19%0.61 ± 2.07%1.27 × 10−4 ± 5.34%0.61 ± 7.18%
1101.57 × 10−5 ± 4.79%0.85 ± 10.20%1.41 × 10−5 ± 6.94%0.51 ± 8.80%
Temperature (°C)k (σR) MDR2k (σR) MDR2
1506.68 × 10−3 ± 9.71%0.56 ± 9.64%7.15 × 10−4 ± 4.56%0.56 ± 12.23%
1305.90 × 10−3 ± 1.43%0.36 ± 5.18%1.92 × 10−4 ± 9.69%0.82 ± 3.84%
1102.63 × 10−5 ± 11.59%0.96 ± 1.05%1.88 × 10−5 ± 5.49%0.83 ± 1.06%
Table 8. Coefficients of aging for the Weidmann model based on DP, εcm, and σR for different insulation oils.
Table 8. Coefficients of aging for the Weidmann model based on DP, εcm, and σR for different insulation oils.
P r o p e r t y   D P ,   ε c m ,   σ R = P r o p e r t y   0   D P ,   ε c m ,   σ R × e x p C p r o p e r t y   T × t
Mineral oil Synthetic ester
Temperature (°C)CDPR2CDPR2
1502.89 × 10−3 ± 10.27%0.31 ± 1.90%1.51 × 10−3 ± 10.04%0.45 ± 4.69%
1301.12 × 10−3 ± 9.60%0.41 ± 6.30%4.81 × 10−4 ± 9.20%0.21 ± 11.35%
1107.28 × 10−5 ± 1.79%0.59 ± 1.24%5.91 × 10−5 ± 2.48%<0.01 ± 9.26%
Temperature (°C)Cεcm CDR2Cεcm CDR2
1504.38 × 10−3 ± 9.57%0.51 ± 2.97%2.56 × 10−3 ± 9.08%0.15 ± 10.81%
1301.86 × 10−3 ± 9.52%0.39 ± 3.32%5.17 × 10−4 ± 9.17%0.61 ± 6.49%
1106.03 × 10−5 ± 6.53%0.96 ± 1.08%3.74 × 10−5 ± 2.11%0.71 ± 8.49%
Temperature (°C)Cεcm MDR2Cεcm MDR2
1503.93 × 10−3 ± 9.27%0.31 ± 1.30%3.22 × 10−3 ± 9.83%0.30 ± 1.70%
1301.83 × 10−3 ± 9.54%0.32 ± 4.41%5.98 × 10−4 ± 7.05%0.38 ± 10.08%
1106.43 × 10−5 ± 6.75%0.53 ± 10.83%4.22 × 10−5 ± 4.14%<0.01 ± 4.20%
Temperature (°C)CσR CDR2CσR CDR2
1502.66 × 10−3 ± 8.03%0.56 ± 6.23%1.31 × 10−3 ± 6.07%0.16 ± 9.48%
1301.19 × 10−3 ± 4.98%0.47 ± 2.70%3.36 × 10−4 ± 6.29%0.45 ± 6.57%
1104.21 × 10−5 ± 8.96%0.68 ± 6.22%3.91 × 10−5 ± 7.35%0.21 ± 4.46%
Temperature (°C)CσR MDR2CσR MDR2
1503.60 × 10−3 ± 9.07%0.27 ± 8.66%2.49 × 10−3 ± 8.63%0.65 ± 2.26%
1301.56 × 10−3 ± 7.68%0.39 ± 1.28%4.36 × 10−4 ± 9.25%0.58 ± 9.59%
1105.81 × 10−5 ± 2.60%0.83 ± 1.66%4.73 × 10−5 ± 10.49%0.59 ± 6.65%
Table 9. Constants for the IEEE model based on lifetime needed to reach end-of-life criteria (DP = 350, εcm = 0.5 ∗ εcm0, σR = 0.5 ∗ σR0) for different insulation oils.
Table 9. Constants for the IEEE model based on lifetime needed to reach end-of-life criteria (DP = 350, εcm = 0.5 ∗ εcm0, σR = 0.5 ∗ σR0) for different insulation oils.
ln L T = A + B / T
Mineral oilSynthetic ester
A (DP)B (DP)R2A (DP)B (DP)R2
9.16 × 10−17 ± 1.15%17,358 ± 2.05%0.92 ± 1.08%9.17 × 10−18 ± 2.85%18,715 ± 2.75%0.99 ± 1.35%
A (εcm) CDB (εcm) CDR2A (εcm) CDB (εcm) CDR2
2.79 × 10−18 ± 3.25%18,648 ± 1.65%0.89 ± 0.95%1.01 × 10−19 ± 1.15%21,883 ± 0.75%0.96 ± 0.85%
A (εcm) MDB (εcm) MDR2A (εcm) MDB (εcm) MDR2
6.55 × 10−16 ± 2.65%16,344 ± 4.20%0.82 ± 1.11%1.57 × 10−21 ± 3.15%21,916 ± 0.97%0.94 ± 2.07%
A (σR) CDB (σR) CDR2A (σR) CDB (σR) CDR2
2.55 × 10−20 ± 1.15%20,637 ± 2.15%0.87 ± 2.07%2.60 × 10−18 ± 2.95%18,982 ± 1.65%0.96 ± 4.24%
A (σR) MDB (σR) MDR2A (σR) MDB (σR) MDR2
3.09 × 10−20 ± 3.65%20,587 ± 3.07%0.90 ± 1.19%3.64 × 10−19 ± 4.08%19,999 ± 3.95%0.99 ± 2.67%
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Fernández-Diego, C.; Ortiz, A.; Carrascal, I.A.; Fernández, I.; Renedo, C.J. Kinetic Assessment of Mechanical Properties of a Cellulose Board Aged in Mineral Oil and Synthetic Ester. Polymers 2021, 13, 4150. https://doi.org/10.3390/polym13234150

AMA Style

Fernández-Diego C, Ortiz A, Carrascal IA, Fernández I, Renedo CJ. Kinetic Assessment of Mechanical Properties of a Cellulose Board Aged in Mineral Oil and Synthetic Ester. Polymers. 2021; 13(23):4150. https://doi.org/10.3390/polym13234150

Chicago/Turabian Style

Fernández-Diego, Cristina, Alfredo Ortiz, Isidro A. Carrascal, Inmaculada Fernández, and Carlos J. Renedo. 2021. "Kinetic Assessment of Mechanical Properties of a Cellulose Board Aged in Mineral Oil and Synthetic Ester" Polymers 13, no. 23: 4150. https://doi.org/10.3390/polym13234150

APA Style

Fernández-Diego, C., Ortiz, A., Carrascal, I. A., Fernández, I., & Renedo, C. J. (2021). Kinetic Assessment of Mechanical Properties of a Cellulose Board Aged in Mineral Oil and Synthetic Ester. Polymers, 13(23), 4150. https://doi.org/10.3390/polym13234150

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop