Next Article in Journal
A Critical Review of Computational Creativity in Built Environment Design
Next Article in Special Issue
Office Distractions and the Productivity of Building Users: The Effect of Workgroup Sizes and Demographic Characteristics
Previous Article in Journal
Most Frequent Problems of Building Structures of Urban Apartment Buildings from 2nd Half of 19th Century and the Start of 20th Century
Previous Article in Special Issue
Critical Review of the Evolution of Project Delivery Methods in the Construction Industry
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Development of Retrofitting Solutions: Remedial Wall Ties for Masonry Enclosure Brick Walls

by
Filipe Rebelo
1,
António Figueiredo
1,
Gonçalo Correia Lopes
1,
Tiago Miguel Ferreira
2,* and
Romeu Vicente
1
1
RISCO, Department of Civil Engineering, University of Aveiro, Campus Universitário de Santiago, 3810-193 Aveiro, Portugal
2
ISISE, Institute of Science and Innovation for Bio-Sustainability (IB-S), Department of Civil Engineering, Campus de Azurém, University of Minho, 4800-058 Guimarães, Portugal
*
Author to whom correspondence should be addressed.
Buildings 2021, 11(1), 28; https://doi.org/10.3390/buildings11010028
Submission received: 17 December 2020 / Revised: 9 January 2021 / Accepted: 11 January 2021 / Published: 13 January 2021
(This article belongs to the Special Issue Buildings: 10th Anniversary)

Abstract

:
The external envelope walls of a significant percentage of the residential building stock in Southern European countries is commonly constituted by infill masonry walls. However, thousands of square meters of this masonry wall typology presents severe issues of cracking and instability, related to the incorrect and deficient support conditions of the outer brick panel of the double-leaf wall solution. In this work, an experimental campaign divided in two phases has been performed to evaluate the effectiveness of two different remedial wall ties retrofitting techniques (Solution A and Solution B) used for double leaf horizontally hollowed clay brick masonry façades. The first phase of the experimental campaign was performed on 120 isolated specimens of horizontally hollowed clay bricks, resorting to post- and pre-NP EN 771-1 brick exemplars (that is, new and pre-existent aged bricks, respectively), as well as on 4 square wallettes, with a side length of 1.20 m, considered as representative of a real scale scenario, for evaluating the two remedial wall ties retrofitting techniques. The second phase of the experimental campaign was performed to fully characterize the different failure types as well as the slipping phenomena observed in the first phase of the experimental campaign, focusing solely on the retrofitting technique Solution B and comprises 24 tests performed on isolated specimens, resourcing to new and pre-existent aged bricks as well. The results obtained by the use of these techniques revealed an average anchorage strength value ranging from 0.25 to 2.5 kN for each tested tie-bar. Solution B reveals an increase of double of the anchorage strength value in comparison to Solution A. In this sense, the global results revealed a suitable applicability of both retrofit studied solutions.

1. Introduction

As a consequence of population and economic growth, an increasing demand for indoor thermal comfort and energy efficiency requirements has arisen, implying new challenges related to buildings’ thermal performance in the European built environment [1]. Thus, during the last few decades, the typology of external infill masonry walls has notably been changing, ranging from the old-fashioned loadbearing massive stone masonry walls into increasingly lighter solutions, in the form of single leaf non-structural brick masonry infills and/or enclosure walls [2].
Although the increasing number of new successful alternative systems for enclosure walls, such as vertically perforated clay bricks [3], double-leaf horizontally hollowed clay brick masonry walls are still one of the most widely used constructive solutions for buildings’ external envelope [2]. These non-loadbearing infill masonry walls are generally supported by a concrete framed structure constituted by columns, beams and slabs, presenting some evident advantages:
When properly and effectively connected, both wall leafs contribute to the global resistance of the wall solution against horizontal actions;
Enables thermal bridge correction solutions, with significant effectiveness in terms of thermal performance;
Enables the protection of the insulation system (when placed within the air gap).
However, since these walls are seldom designed to withstand severe external loads but rather to perform an infilling function, their design is often neglected and insufficiently detailed [4]. Moreover, in addition to the non-structural pathological defects associated with infill masonry walls (generally comprising loss of water tightness, mould growth and the development of condensation issues), distortions may occur as well as excessive deformation as consequence of hygrothermal movements, leading to severe cracking or even to its collapse, compromising not only the buildings serviceability and functionality, but most importantly human life [5,6,7].
Concerning the critical role of buildings’ external envelope walls in terms of protection from the environmental elements whilst assuring desirable indoor thermal comfort conditions to the building occupants, one of the most debatable measures in terms of constructive systems solutions has been the external thermal bridge correction by means of clay brick slips or veneer cladding, aligned with the underlying strategy of the European Union (EU) energy policy framework for reducing the environmental impacts and the ecological footprint, as well as to reduce energy consumption through improving energy efficiency in buildings without compromising the living quality standards [8,9]. Despite these constructive systems solutions contributing to the improvement of the buildings’ façade thermal behavior, insufficient testing and technological validation has been responsible for a considerable amount of pathologies associated with deficient support conditions, and therefore severe cracking and instability of horizontally hollowed clay brick enclosure infill masonry walls have been observed. In Figure 1a, it is depicted how the disrespect of the rule to maintain a minimal partial width support over the concrete beam of at least 2/3 of the outer wall leaf, in accordance to [10], has led to numerous severe issues, imposing in some situations the demolition and re-construction of the external leaf of the wall [6,7].
Additional contributing factors responsible for cracking and instability problems observed in several buildings have been identified as the excessive weight of the exterior rendering, additional eccentric loads, wind loads, creep and shrinkage movements of the structure, masonry deformations and movements induced by heat and moisture, lack of wall ties, lack of building technology knowledge in the design phase, and non-specialized workmanship skills (particularly for singular points) [7].
When subjected to seismic actions, despite the masonry enclosure and infills walls being considered non-structural, several authors [7,11,12,13] have acknowledged their influence on the global behavior of the reinforced concrete frames under seismic loads, considering that their disregard in the design process of new buildings may induce local mechanisms in the structure. The abovementioned phenomena has recently been observed as consequence of several earthquake events, as referred to by [14]. Consequently, the lessons learnt about the influence of the non-structural masonry enclosure and infills walls on the buildings’ structural response under seismic action have been the basis for important improvements of several structural design standards [15,16,17,18,19].
It should also be mentioned that the reduced wall support usually required to minimize thermal bridges due to structural elements is an issue when the building is subjected to seismic actions, since these masonry enclosure and infill walls exhibit a non-desirable and fragile out-of-plane behavior, resulting in the manifestation of severe cracking, which, in the worst case scenario, is responsible for the walls to completely detach and collapse, as observed in Figure 1b. Considering that the associated costs involved in repairing non-structural elements often exceeds the structural repair ones [7,14,20], the need to study and evaluate suitable measures in order to improve and assure the in-plane and out-of-plane integrity of enclosure and infill masonry walls, possibly subjected to seismic actions, is paramount to minimize the adverse consequences.
Several strengthening intervention methods and retrofitting techniques applied in masonry enclosure and infill walls have been extensively addressed in the literature, such as the use of fibre reinforced polymers (FRP), engineered cementitious composites (ECC), textile reinforced mortars (TRM) and ferrocement and bed joints’ reinforcement [4,21,22,23,24].
The present paper focuses on the using of the remedial wall tying retrofitting technique (by means of different techniques comparison), originally developed for Northern European clay brick veneer wall systems [25], and therefore adapted to the Southern European traditional horizontally hollowed clay brick masonry walls. Based on the experimental investigation herein presented, conduced within two different techniques—that is, Solution A based on the insertion of a remedial helicoidal tie through percussion, and Solution B based on the use of a cement grout sock on the extremities of the remedial wall tie—the effectiveness and adequacy of using this technique in real retrofitting interventions will be thoroughly discussed in the following sections. To achieve the specific objective of fully assessing the adequacy and efficiency of the presented post-construction pinning techniques in future real retrofitting interventions, the experimental work presented in this paper comprises the following steps: (i) assess the retrofitting technique in laboratorial environment; (ii) evaluate the efficiency of the retrofitting solution on specimens constituted by post- and pre-NP EN 771-1 horizontally hollowed clay bricks (meaning, resourcing to new and pre-existent aged brick exemplars); (iii) evaluate the influence of different features of the retrofitting technique (such as sleeve introduction and grout injection) over the pull-out test results; and, finally, (iv) describe and catalogue the different failure types and the observed behavior of the two different techniques tested. Resourcing to new and pre-existent aged horizontally hollowed clay brick exemplars for testing purposes has been considered paramount to assess behavior and performance differences, since aged bricks (pre-NP EN 771-1) have already been exposed to different humidity, moisture and temperature conditions, therefore experiencing innumerable cycles of temperature charge and discharge, no longer comprising the initial (as when new) physical, chemical and mechanical characteristics, allowing this way the simulation of an approximated scenario to real post-construction retrofitting environment conditions. On the other hand, new horizontally hollowed clay bricks (post-NP EN 771-1) are expected to behave according to their optimal physical and mechanical characteristics. The results acquired for both retrofitting techniques are thoroughly presented and discussed.

2. Wall Tie Retrofitting Techniques

One of the techniques used during the construction process, specifically aimed at avoiding defects related to the lack of adequate support of the outer brick wall layer (see Section 1), has often been the use of steel wall ties, embedded into the mortar layers to connect the two brick wall leafs as well as for connecting the walls to confining and adjacent structural elements, such as concrete columns. However, the location of these steel connectors is frequently random and the wall ties are often inappropriate, revealing to be fragile, prone to corrosion and unable to aid draining internal condensation in the wall cavity [26].
The post-construction remedial wall tying arises therefore as one of the suitable retrofitting techniques, able of being successfully applied for these type of constructive solution for walls, improving its out-of-plane integrity as well as stability [27]. Among all of the solutions available in the construction market, this paper focuses on the comparative analysis of two particular solutions applied to horizontally hollowed clay brick cavity walls, hereinafter referred to as Solution A (as depicted in Figure 2a) and Solution B (as depicted in Figure 2b). Solution A is a based on the insertion of a remedial helicoidal tie that is inserted through percussion and connects the two wall leafs solely by friction. Solution B is based on the insertion of cement grout sock that constitutes an anchoring bulb on the extremities of the remedial wall tie.
The choice for these two solutions was motivated by the fact that they both present advantageous features (presented in Table 1) and have been applied extensively in retrofitting across Europe.
From the comparison between the two solutions, it is noteworthy that Solution A is expected to be a more economic tie solution, does not require skilled workmanship and presents higher productivity levels since it allows the execution of a larger number of ties in a shorter period of time. However, Solution B tends to be a more effective tie solution since the use of grout bulbs results in higher tensile strengths, but nevertheless comprises higher material costs, and since a curing period is mandatory, the process becomes slightly more time-consuming.

3. Methodology

The developed work of the experimental campaign performed in the scope of this study follows the methodological approach depicted in the schematic flowchart presented in Figure 3.
The work methodology is structured into two main phases, preceded by the geometric and mechanical properties characterization of the horizontally hollowed clay bricks to be used throughout the experimental campaign. The first phase of the experimental campaign was performed on 120 isolated specimens (depicted in Figure 6a) of horizontally hollowed clay bricks, resorting to post- and pre-NP EN 771-1 [28] brick exemplars (that is, new and pre-existent aged bricks, respectively, as explained in Section 1), meaning that a total of 120 specimens, divided in 30 specimens composed of new bricks and 30 specimens composed of pre-existent aged bricks for studying Solution A, and 30 specimens composed of new bricks and 30 specimens composed of pre-existent aged bricks for evaluate Solution B, were tested and each individual response has been assessed. Additionally, 4 square wallettes were constructed with a side length of 1.20 m (as depicted in Figure 6b) and tested for evaluating the two remedial wall ties retrofitting techniques (Solution A and Solution B). The second phase of the experimental campaign was performed to fully characterize the different failure types as well as the slipping phenomena observed in the first phase of the experimental campaign, focusing solely on the retrofitting Solution B and comprises 24 tests performed on isolated specimens, resourcing to new and pre-existent aged bricks as well. Therefore, a series of compression tests have been performed according to the procedure presented in NP EN 772-1 [29] for mechanical characterization of the clay bricks. As for the two phases of the experimental campaign, a series of pull-out tests have been performed for both the isolated specimens and the wallettes, whose results obtained have been registered and discussed throughout the respective subsections.

4. Characterization of the Clay Bricks

Two double-leaf cavity wall masonry specimens composed of two different formats of horizontally hollowed clay bricks were constructed and tests were performed for studying a common constructive solution, as referred to in the Introduction (see Section 1), considered to be representative of the majority of the building envelope walls existing in Southern European built environment. In order to enrich the discussion, two distinct frameworks were considered: pre- and post-European Standard NP EN 771-1 [28], in which the physical and mechanical features of the masonry units as well as its geometric tolerances are specified. In this sense, prior to the construction of the specimens, bricks used were geometrically and mechanically characterized according to the recommendations of the European Standard NP EN 772-1 [29]. The obtained results for the performed characterization are presented and discussed throughout the following subsections.

4.1. Geometrical Characterization

The geometrical characterization of the specimens was evaluated, based on a randomly selected group of six horizontally hollowed clay brick exemplars. The nomenclature used for the brick types is based on their representative measures (in (cm) unless otherwise stated) of 30 × 20 × 15 and 30 × 20 × 11 (meaning: Length × Height × Width), as depicted in Figure 4, both compliant with pre- and post-NP EN 771 1 [28] requirements. Regarding to length and height, the 30 × 20 × 15 and 30 × 20 × 11 bricks can present significant dimensional variations, ranging between 28.8 cm to 30.2 cm and between 18.4 cm and 19.6 cm, respectively. In the same line, in terms of width, the 30 × 20 × 15 bricks can present dimensions ranging from 14.5 cm to 15.5 cm, while the 30 × 20 × 11 bricks can present dimensional variations ranging between 10.6 cm and 11.4 cm. The thickness of the bricks’ wall and webs range from 0.8 cm to 1.0 cm.

4.2. Mechanical Characterization

The mechanical characterization of the horizontally hollowed clay brick specimens have been performed by means of a series of simple compression tests, complying with the standard procedure presented in EN 772 1 [29]. The acquired average values from the tests performed for the six bricks of each type, as well as the corresponding coefficients of variation are presented in Table 2. The compressive strength values of the Pre-NP EN 771-1 bricks are slightly higher due to the thicker inner septums/webs.
During the execution of the tests performed for mechanical characterization, four main types of failure were registered: detachment of the outer webs of the brick, global crushing, cracking of the inner webs and fractional shear. The four failure types were registered and presented in Figure 5.

5. Experimental Campaign: Phase 1

The aim of the first phase of the experimental campaign has been to test the two distinct previously selected solutions of post-construction wall tying (that is, Solution A and Solution B), with the specific objective of evaluating its efficiency and to understand the main differences between the both solutions, in terms of mechanical behavior and execution procedure by means of material use and time consumption related to each application process. Considering these objectives, a total of 120 specimens (divided in 30 for each solution and for each one of the two sets of specimens, as explained in Section 3), were tested and each individual response has been assessed. Additionally, to evaluate the two post-construction wall tie techniques, four scaled specimens of masonry wallettes were constructed.

5.1. Preparation of the Test Specimens

The specimens were built and prepared following an assembly line analogy (depicted in Figure 6a). The specimen preparation started with the placement of the 30 × 20 × 11 bricks. Secondly, polystyrene bars (XPS), previously prepared, were carefully placed on top of the first layer of bricks (see Figure 6a and Figure 7), to simulate the air-gap space between layers. Finally, the specimen has been “closed” with the placement of the 30 × 20 × 15 brick panel. To assure the functioning of the system and the correct application of the post construction wall tie, a set of wood boards and clamps were used to guarantee the stability of the bricks during the drilling process and the application of the solutions.
Regarding the four masonry wallettes (see Figure 6b), their construction followed a similar sequence: (i) preparation of the brick laying mortar; (ii) positioning of the first row of bricks; (iii) pre-wetting of the bricks; (iv) brick laying; (v) filling of the vertical head mortar joints; and (vi) rendering of the masonry wallettes.

5.2. Application of the Post-Construction Wall Tying for Single Isolated Specimens

5.2.1. Solution A

For the application of Solution A, the used steel tie rods were made of stainless steel with a helical format of 8 mm in diameter. As observable in Figure 8a, the first step consisted of pre-drilling the bricks resorting to a 5 mm drill. Secondly, the helical tie rods were placed into the pre-drilled holes, as seen Figure 8b. Regarding this procedure, it is worth mentioning that the insertion of the tie rods have been performed by crimping, i.e., by drilling with pulse, resorting to an adaptor coupled to the drill, specifically for this purpose.

5.2.2. Solution B

For the application of Solution B, special care has been taken during the insertion and positioning of the sleeves (either sock or plastic), necessary for the application of the grout. Otherwise, these jacks tend to be placed in an incorrect manner, leading either to the malfunctioning of the grout or making impossible its injection. It is worth noting that the injection is itself a particularly demanding task to perform, since its application has been made with the grout injection nozzle gun positioned vertically, making it difficult to control the grout introduction. Another important aspect that must be considered in this solution is the required curing time of the grout (28 days in the particular case of a cement-based grout). The execution steps followed for the application of Solution B are presented in Figure 9.

5.3. Application of Post Remedial Wall Ties on the Masonry Wallettes

The application of post remedial wall ties on the masonry wallettes has followed the same procedure used on the preparation of the isolated specimens. Particular precaution has been taken prior to drilling on the positioning of holes in order to avoid hitting the vertical head mortar joints. Additional concern considered during the implementation of this solution has been to assure that the adequate amount of grout was injected into each sock sleeve, in order to guarantee the formation of a suitable bulb. The shape of the grout bulb formed is independent of the direction of the grout injection. For the sake of comparison, this was verified before defining the first experimental testing procedure, when the injection was done for the two brick specimens (single isolated specimen) in the vertical direction and for the double leaf wall specimen in the horizontal direction. In both cases, the “egg” shaped grout bulb has always been formed because of two reasons: (i) the consistency of the injected grout, that is not excessively fluid; and (ii) the flexible sock that restrains and prevents an irregular shaped bulb from being formed.

5.4. Description of the Pull-Out Tests

For the singular isolated specimens, the helical steel rod has been cut between both bricks (that is, in the air gap existing between the two brick panels), since this testing approach intends to pull-out the steel rods individually. The test has been performed resourcing to a 3 kN dynamometer for precision purposes. Regarding the wallette specimens, aiming to reproduce a real wall in a laboratory environment, they were constructed to test and identify pinning application constraints, limitations, as well as improvement measures for both techniques. For Solution A pull-out tests performed, a 3 kN dynamometer has been used, and for Solution B, a 16 kN dynamometer was used to take advantage of the resolution and precision of the equipment since, in the case of the pull-out tests for Solution B, these exceed the value of 3 kN.
A noteworthy aspect related to the testing set-up is that, in order to inject the grout into the sock sleeve, due to their additional extension, it was necessary to arrange an adapter for placing the injection gun, making it possible to apply the grout within the inner sock sleeve inserted into the 30 × 20 × 15 brick.

5.5. Analysis of the Results Obtained in the First Testing Campaign

5.5.1. Solution A

As previous referred to in Section 4, all the single brick specimens (including both new and pre-existent bricks) were tested according to the procedure defined in the standard NP EN 771-1 (CEN2006). Following to the methodology described in Section 3, the specimens were tested in pull-out and the record of relevant information from the tests, namely, load cell forces were collected and presented in Figure 10. From the results obtained, it is shown that pre-existent brick specimens (designated in the plots as #cm ExiB, meaning, dimension of the brick type and pre-existent specimen) present, on average, a higher pull-out force in respect to new brick specimens (designated in the plots as #cm NewB, meaning dimension of the brick type and new specimen); and for new and pre-existent specimens of 30 × 20 × 15 brick type format, this force is higher with respect to the 30 × 20 × 11 brick format. Since Solution A is strictly dependent on frictional force mobilization of the helical steel bar, these results were somehow expectable considering the brick geometry of hollows and web thickness, higher in the case of the 30 × 20 × 15 bricks. When compared with the new specimens, pre-existent bricks present higher compressive strength (indicator of better mechanical behavior), and the thicker value of the webs is also higher, leading therefore to higher pull-out force in both formats. In addition, since brick formats 30 × 20 × 15 have three webs that are pierced, in respect to the two of the 30 × 20 × 11 brick format, higher frictional resistance is expected and consequently the pull-out values for the wider bricks are higher. The result values obtained for the pull-out tests performed in the wallettes were, on average, higher when compared with the obtained results for the single brick specimens.
From the analysis of Figure 10, it is possible to observe—even though taking into account the difference in the testing methodology for the single brick specimens, for which the pull-out tests are done individually for each brick—that the pull-out force of the 30 × 20 × 15 brick format is 20% to 50% higher than the one of the 30 × 20 × 11 format. Comparing the pull-out forces obtained of the wallette and the 30 × 20 × 15 brick format, an increase between 40% to 95% was attained for the pull-out force in the wallette specimens, proving that the mechanical pinning between bricks is beneficial for this type of horizontally hollowed brick geometry. However, further testing driven to better understand this relationship is encouraged.
From the analysis of Figure 11 it is possible to observe that pre-existent bricks specimens present, on average, higher compressive strength, when compared with new brick specimens. Thus, a direct correlation was observed in the attained results (compression and pull-out force), showing the same tendency of higher result values for the existent brick specimens. Finally, regarding the failure mode, all tests revealed that in Solution A, when applied to the wallettes, failure occurs exclusively by steel tie slippage.

5.5.2. Solution B

As previous referred to in Methodology (see Section 3), the testing framework and the number of specimens for Solution B was the same used for Solution A.
From the analysis of Figure 12, it is possible to conclude that both new and the pre-existing bricks specimens present higher pull-out force values for the specimens with 30 × 20 × 15. Although the closed-end sock sleeve inserted into the inner leaf of the 30 × 20 × 11 brick may, at first sight, allow a better formation of the grout bulb (due to the assured pressure of the grout injection nozzle gun), its effectively formed contact area between the grout bulb and the web of the brick may still be reduced. Furthermore, the fact that the sock sleeve, inserted into the outer leaf of the 30 × 20 × 15 brick, is opened on both extremities (since the helical steel bar must pass through) and pierces two webs of the brick, may even be positive to the formation of one smaller additional bulb after the first inner web, leading to improved results.
The results obtained for the pull-out tests performed on the wallette specimens (new and pre-existent bricks) are depicted in Figure 12. The acquired results reveal that the pull-out force of the wallette is about 5% to 15% higher when compared with the force attained for the 30 × 20 × 15 brick specimens.
Regarding the comparison between the compressive strength results with the pull-out forces, as depicted in Figure 13, Solution B do not exhibit the same tendency observed in Solution A, attaining higher values of the pull-out force when the compressive strength is also higher. In this sense, only the 30 × 20 × 15 specimens reveals higher resistance in the pull-out tests when the compressive strength is higher as well. In opposition of Solution A, this wall tie execution technique strongly depends on other features, such as the grout quality and bulb formation into the hollowed bricks, tie insertion or bond to the grout, and, most importantly, on the quality of the execution, as will be discussed further.
From the pull-out tests performed on the specimens using Solution B, it was possible to identify three types of failure modes:
  • Fragile failure (FF): this type of failure appears when, during the test, abrupt loss of adhesion occurs between the tie-bar and the brick walls/webs, driven by the loss of strength capacity of the brick to the pull-out force. Figure 14a presents an example of this failure, conditioned by the brick resistance.
  • Failure by tie-bar slippage (FTS): this type of failure arises when slippage of the tie-bar occurs within the grout. From Figure 14b, it is possible to verify that the brick web is intact without attaining the failure, and the sock sleeve is not moved from the initial position.
  • Global failure (GF): this type of failure occurs when the brick gradually weakens and fails, and the system solution (sleeve plus tie) slides along the brick web. In Figure 14c, it is observed the slippage of the solution relative to the hollowed brick web. It is also quite noticeable the slipping experienced once the initial position of the sock sleeve nears the right exterior web of the brick.

6. Experimental Campaign: Phase 2

The second phase of the experimental campaign was developed to fully characterize the different failure types as well as the slipping phenomena attained in the previously phase of the experimental campaign. This second phase comprises 24 tests performed in isolated specimens from Solution B using new and pre-existent bricks. It is noteworthy that the preparation of the specimens and the application of the reinforcement wall tie solution have followed the procedure adopted for the first phase of the experimental campaign, previously described in Section 3 and Section 5.
Regarding the pull-out tests, this second phase was performed with a different experimental setup, consisting of the use of a hydraulic jack of 300 kN, fixed to a steel frame coupled to a load cell with capacity of 25 kN in traction and compression (see Figure 15) that has been used to perform the experimental tests. At the top of the load cell, a steel grip was placed to clamp the steel helical tie (see Figure 15b). The specimens were constrained by a steel sheet fixed in the outer corners to the lower beam of the steel frame setup (Figure 15d).
At this experimental campaign, the tests were performed with the two bricks connected by the tie (see Figure 7). Thus, it allowed to attain the value of the pull-out strength of the entire solution. Finally, the tests were performed at a constant speed with a rate of 0.2 mm/s controlled by the displacement transducer of the hydraulic jack.
Based on the obtained results, individual plots (i.e., by specimen) of the pull-out strength vs. displacement recordings were generated considering the registered behavior in terms of strength evolution, slipping and global displacement. Table 3 presents the behaviors registered for three groups of new brick specimens tested (a representative test was chosen as example for each group of tests and it is depicted in the plot), whereas Table 4 presents the result for the two groups of pre-existent brick specimens.
In summary, and regarding the tests performed on new brick specimens, it has been possible to identify three types of failure modes:
  • Failure by tie slippage (FTS): approximately constant pull-out force during the test, and abrupt decrease in strength in the rupture;
  • Global failure (GF): the variation of the pull-out force during the test clearly indicates the instant when yielding occurs at each web of the bricks;
  • Fragile failure (FF): after the maximum value of the pull-out force is attained and yielding occurs, the specimen no longer has the capacity to attain pull-out strength values similar to the maximum peak of strength.
In summary, it was possible to identify two types of failure modes for the pre-existent brick specimens:
  • Failure by tie slippage (FTS): as in the previous group of new brick specimens, this type of failure was obtained;
  • Brittle failure (BF): the pull-out force does not reach values higher than the maximum previously obtained.
Regarding the quality control, as stated above in Section 5.2.2, special attention should be given to the grout injection process, as it strongly influences the effectiveness of the solution. However, there are other parameters presented to control, such as the grout workability time and preparation, which should have an adequate fluidity so that it can be easily injected in the sock sleeve. Another important factor that must be adequately controlled is the drilling process, which requires a careful execution to avoid undesirable damages in the bricks as well as to avoid undermining the steps to be carried out afterwards. Thus, a perpendicular drilling stance is mandatory to allow the introduction of the sock sleeves avoiding extra damages to the specimens. It is also important to control the drilling depth, since it is necessary to preserve the last web of the brick of the internal leaf (usually concerning the 30 × 20 × 11 brick format in the case of a double-leaf wall).
Regarding the execution of the sock sleeves strengthening technique piercing the brick, it should also be thoroughly controlled, since the risk of tearing the sock sleeves when passing through the webs or becoming deformed is possible.

7. Conclusions

This paper focused on the effectiveness of two different remedial wall ties retrofitting techniques with the purpose of tackling a recurrent problem concerning the instability of double-leaf masonry enclosure walls.
The potential advantages offered by the two studied solutions have proven the suitability and reliability of these retrofitting techniques to connect both wall leafs effectively, thus contributing to the global resistance of the existent wall solution against horizontal actions. Due to frequent deficient support conditions of the external envelope layer, the need of adequate connection between the two masonry wall leafs is crucial to mitigate the risk of collapse due to excessive deformation or seismic actions, ultimately compromising human life [31,32].
The work comprised an experimental campaign divided into two phases, preceded by the geometric and mechanical characterization of the horizontally hollowed clay bricks (30 × 20 × 15 and 30 × 20 × 11, new and pre-existent aged bricks) used throughout the study. To characterize the effectiveness of the remedial wall tie solutions, a total of 120 isolated specimens and 4 wallettes were executed and tested by performing the pull-out technique. Two different retrofit scenarios have been tested and compared, analyzing two solutions. Solution A is a based on the insertion of a remedial helicoidal tie that is inserted through percussion and connects the two wall leafs solely by friction. Solution B is based on the insertion of cement grout sock that constitutes an anchoring bulb on the extremities of the remedial wall tie.
From the attained results from Phase 1 of the experimental campaign, it is possible to conclude that pre-existent bricks specimens present higher compressive strength as well as pull-out force, when compared with new brick ones, revealing a direct correlation. Regarding the failure modes, all tests revealed that in Solution A, when applied to the wallettes, the failure occurs exclusively by steel tie slippage.
The technique of Solution B is strongly dependent on the grout quality and bulb formation into the hollowed bricks, tie insertion or bond to the grout, and on the quality of the execution.
The second phase of the experimental campaign revealed that no coherent rupture type was attained. In this sense, three different types of rupture have been observed, namely “failure by tie slippage” characterized by a constant value for pull-out force followed by an abrupt decrease in strength; “global failure,” in which the pull-out test behavior reveals a swing of the applied force, until the rupture occurs; and “fragile failure,” where after the maximum value of the pull-out force is attained and yielding occurs, the specimen no longer has the capacity to attain pull-out strength values similar to the maximum peak of strength. This research has opened the discussion on various levels, starting from the need to rethink the technology and execution rules of facades and development of execution guidelines, especially in the cases of veneer wall solutions and erection of infill walls in seismic prone areas, as well as in the case of retrofitting to lead the way to the development of optimization these retrofitting approaches in terms of intervention cost-technical benefit.

Author Contributions

All the authors have contributed in multiple tasks throughout this research. Specifying the individual contributions: Conceptualization: F.R., A.F., G.C.L., T.M.F. and R.V.; methodology: F.R., A.F., T.M.F. and R.V.; software, A.F., T.M.F., R.V.; validation: F.R., A.F., G.C.L., T.M.F. and R.V.; formal analysis: F.R., A.F., G.C.L., T.M.F. and R.V.; investigation: F.R., A.F., G.C.L., T.M.F. and R.V.; resources: F.R., A.F., G.C.L., T.M.F. and R.V.; data curation: F.R., A.F., G.C.L., T.M.F. and R.V.; writing—original draft preparation: F.R., A.F., G.C.L., T.M.F.; writing—review and editing: F.R., A.F., G.C.L., T.M.F. and R.V.; visualization: T.M.F. and R.V.; supervision: T.M.F. and R.V.; project administration: T.M.F. and R.V.; funding acquisition: T.M.F. and R.V. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Informed Consent Statement

Not applicable. (Study not involving humans).

Data Availability Statement

The data presented in this study are available on request from the corresponding author. The data are not publicly available since this research work is still ongoing with the development of additional solutions based on the attained results.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Lee, J.H.; Yeo, M.-S. Condensation Control to Cope with Occupancy Activity and Effectively Mitigate Condensation in Unheated Spaces by Real-Time Sensor Control Strategy. Sustainability 2020, 12, 4033. [Google Scholar] [CrossRef]
  2. Teni, M.; Krstić, H.; Kosiński, P. Review and comparison of current experimental approaches for in-situ measurements of building walls thermal transmittance. Energy Build. 2019. [Google Scholar] [CrossRef]
  3. Lourenço, P.; Vasconcelos, G.; Medeiros, P.; Gouveia, J. Vertically perforated clay brick masonry for loadbearing and non-loadbearing masonry walls. Constr. Build. Mater. 2010, 24, 2317–2330. [Google Scholar] [CrossRef]
  4. Furtado, A.; Rodrigues, H.; Arêde, A.; Varum, H. Experimental tests on strengthening strategies for masonry infill walls: A literature review. Constr. Build. Mater. 2020. [Google Scholar] [CrossRef]
  5. Silva, L.M.; Marting, A.; Vasconcelos, G.; Lourenço, P.B. Paredes de Alvenaria de Fachada: Soluções e Sugestões de Melhoria de Desempenho. In Proceedings of the Seminário de Reabilitação de Fachadas, Guimarães, Portugal, 22 September 2016. [Google Scholar]
  6. Vicente, R.; Da Silva, J.A.R.M. Defects of non-loadbearing masonry walls due to partial basal supports. Constr. Build. Mater. 2007, 21, 1977–1990. [Google Scholar] [CrossRef]
  7. Vicente, R.; Rodrigues, H.; Varum, H.; Costa, A.; Da Silva, J.A.R.M. Performance of masonry enclosure walls: Lessons learned from recent earthquakes. Earthq. Eng. Eng. Vib. 2012, 11, 23–34. [Google Scholar] [CrossRef]
  8. Directive 2018/844/EU of the European Parliament and of the Council of 30 May. Off. J. Eur. Union 2018, 156, 75–91.
  9. Figueiredo, A.; Rebelo, F.; Castanho, R.A.; Oliveira, R.; Lousada, S.; Vicente, R.; Ferreira, V. Implementation and Challenges of the Passive House Concept in Portugal: Lessons Learnt from Successful Experience. Sustainability 2020, 12, 8761. [Google Scholar] [CrossRef]
  10. Groupe de Coordination des Textes Techniques. Parois et Murs en Maçonnerie de Petits Éléments; DTU 20.1 (référence AFNOR DTUP10-202); Centre Scientifique et Technique du Bâtiment: Marne-la-Vallée, France, 1985. [Google Scholar]
  11. Furtado, A.; Rodrigues, H.; Arêde, A.; Varum, H. Simplified macro-model for infill masonry walls considering the out-of-plane behaviour. Earthq. Eng. Struct. Dyn. 2016, 45, 507–524. [Google Scholar] [CrossRef]
  12. Crisafulli, F.J.; Carr, A.J.; Park, R. Analytical modelling of infilled frame structures—A general review. Bull. New Zeal. Soc. Earthq. Eng. 2000, 33, 30–47. [Google Scholar] [CrossRef] [Green Version]
  13. Rodrigues, H.; Varum, H.; Costa, A. Simplified Macro-Model for Infill Masonry Panels. J. Earthq. Eng. 2010, 14, 390–416. [Google Scholar] [CrossRef]
  14. The L’Aquila, Italy Earthquake of 6 April 2009—A Preliminary Field Report by EEFIT; EEFIT: London, UK, 2009.
  15. Eurocode 8: Design of Structures for Earthquake Resistance—Part 1: General Rules, Seismic Actions and Rules for Buildings 2004; European Committee for Standardization: Brussels, Belgium, 2004.
  16. Eurocode 6: Design of Masonry Structures—Part 11: General Rules for Reinforced and Unreinforced Masonry Structures 2005; European Committee for Standardization: Brussels, Belgium, 2005.
  17. NEHRP Handbook for the Seismic Evaluation of Existing Buildings—A Prestandard, Federal Emergency; FEMA 310; Federal Emergency Management Agency: Washington, DC, USA, 1998.
  18. Seismic Evaluation and Retrofit of Concrete Buildings—Technical Report; ATC-40; Applied Technology Council: Redwood City, CA, USA, 1996.
  19. Assessment and Improvement of the Structural Performance of Buildings in Earthquakes; New Zeland Society for Earthquake Engineering: Wellington, New Zeland, 2006.
  20. Earthquake Hazard Mitigation for Nonstructural Elements—Field Manual; FEMA 74; Federal Emergency Management Agency: Washington, DC, USA, 2005.
  21. Özgür, A.; Tatayoğlu, M.; Demirhan, M. Out-of-plane behavior of unreinforced masonry brick walls strengthened with CFRP strips. Constr. Build. Mater. 2012, 35, 614–624. [Google Scholar] [CrossRef]
  22. Chen, W.; Yeh, Y.-K.; Hwang, S.-J.; Lu, C.-H.; Chen, C.-C. Out-of-plane seismic behavior and CFRP retrofitting of RC frames infilled with brick walls. Eng. Struct. 2012, 34, 213–224. [Google Scholar] [CrossRef]
  23. Ozsayin, B.; Yilmaz, E.; Ispir, M.; Ozkaynak, H.; Yüksel, E.; Ilki, A. Characteristics of CFRP retrofitted hollow brick infill walls of reinforced concrete frames. Constr. Build. Mater. 2011, 25, 4017–4024. [Google Scholar] [CrossRef]
  24. Kesner, K.; Billington, S.L. Investigation of Infill Panels Made from Engineered Cementitious Composites for Seismic Strengthening and Retrofit. J. Struct. Eng. 2005. [Google Scholar] [CrossRef]
  25. Memari, A.M.; Burnett, E.F.; Kozy, B.M. Seismic response of a new type of masonry tie used in brick veneer walls. Constr. Build. Mater. 2002, 16, 397–407. [Google Scholar] [CrossRef]
  26. Graça, J. Intervenções em Fachadas: Novas Soluções Para Problemas Antigos. In Proceedings of the Seminário de Reabilitação de Fachadas, Guimarães, Portugal, 22 September 2016; pp. 73–82. [Google Scholar]
  27. Mendes da Silva, J.A.R.; Carvalhal, M.; Vicente, R.D.S. Reforço mecânico de alvenaria de tijolo: Reabilitação de cunhais e grampeamento metálico pós-construção. In Proceedings of the Encontro Sobre Conservação e Reabilitação de Edifícios, Lisboa, Portugal, 26–30 May 2003; pp. 1329–1338. [Google Scholar]
  28. Specification for Masonry Units—Part 1: Clay Masonry Units; NP EN 771-1; European Committee for Standardization: Brussels, Belgium, 2006.
  29. Methods of Test for Masonry Units—Part 1: Determination of Compressive Strength; NP EN 772-1; European Committee for Standardization: Brussels, Belgium, 2002.
  30. Ribeiro, S. Soluções de Reabilitação—Grampeamento de Paredes de Alvenaria. Master’s Thesis, University of Aveiro, Aveiro, Portugal, 2013. [Google Scholar]
  31. Aguado, J.L.P.; Ferreira, T.M.; Lourenço, P. The Use of a Large-Scale Seismic Vulnerability Assessment Approach for Masonry Façade Walls as an Effective Tool for Evaluating, Managing and Mitigating Seismic Risk in Historical Centers. Int. J. Arch. Herit. 2018, 12, 1259–1275. [Google Scholar] [CrossRef]
  32. Ferreira, T.M.; Maio, R.; Costa, A.A.; Vicente, R. Seismic vulnerability assessment of stone masonry façade walls: Calibration using fragility-based results and observed damage. Soil Dyn. Earthq. Eng. 2017, 103, 21–37. [Google Scholar] [CrossRef]
Figure 1. Examples of severe mechanical pathologies as consequence of: (a) inadequate correction of thermal bridges, using partially supported infill walls; (b) cracking and out of plane collapse of outer leaf of double-leaf cavity walls and veneer cladding walls [7].
Figure 1. Examples of severe mechanical pathologies as consequence of: (a) inadequate correction of thermal bridges, using partially supported infill walls; (b) cracking and out of plane collapse of outer leaf of double-leaf cavity walls and veneer cladding walls [7].
Buildings 11 00028 g001aBuildings 11 00028 g001b
Figure 2. Functioning scheme of the two solutions considered: (a) Solution A—dry remedial wall tie in horizontally hollowed bricks; (b) Solution B—remedial wall tie using an expanded grout-filled sock in horizontally hollowed bricks.
Figure 2. Functioning scheme of the two solutions considered: (a) Solution A—dry remedial wall tie in horizontally hollowed bricks; (b) Solution B—remedial wall tie using an expanded grout-filled sock in horizontally hollowed bricks.
Buildings 11 00028 g002
Figure 3. Flowchart diagram of the work methodology for the experimental campaign.
Figure 3. Flowchart diagram of the work methodology for the experimental campaign.
Buildings 11 00028 g003
Figure 4. Formats of the horizontally hollowed clay bricks used in the experimental tests: (a) 30 × 20 × 15; and (b) 30 × 20 × 11.
Figure 4. Formats of the horizontally hollowed clay bricks used in the experimental tests: (a) 30 × 20 × 15; and (b) 30 × 20 × 11.
Buildings 11 00028 g004
Figure 5. Types of failure observed: (a) detachment of the outer webs; (b) global crushing; (c) cracking of the inner webs; (d) fractional shear.
Figure 5. Types of failure observed: (a) detachment of the outer webs; (b) global crushing; (c) cracking of the inner webs; (d) fractional shear.
Buildings 11 00028 g005
Figure 6. Test specimens and wallettes: (a) preparation of the isolated specimens; (b) masonry wallettes, adapted fom [30].
Figure 6. Test specimens and wallettes: (a) preparation of the isolated specimens; (b) masonry wallettes, adapted fom [30].
Buildings 11 00028 g006
Figure 7. Schematic detail of an isolated specimens: (1) Steel tie rod; (2) 30 × 20 × 15 brick; (3) 30 × 20 × 11 brick; (4) XPS insulation bar.
Figure 7. Schematic detail of an isolated specimens: (1) Steel tie rod; (2) 30 × 20 × 15 brick; (3) 30 × 20 × 11 brick; (4) XPS insulation bar.
Buildings 11 00028 g007
Figure 8. Solution A execution process: (a) pre-drilling of the brick; (b) crimping the steel rod into the brick.
Figure 8. Solution A execution process: (a) pre-drilling of the brick; (b) crimping the steel rod into the brick.
Buildings 11 00028 g008
Figure 9. Solution B step-by-step execution process: (a) pre-drilling of the bricks with a 5 mm drill; (b) drilling of the bricks with a 14 mm drill; (c) placement of the closed-end sock sleeve into the 30 × 20 × 11 brick (inner brick); (d) filling of the sock sleeve with the cement based grout; (e) placement of the helical tie rod into the hole and the outer brick sock sleeve; (f) sock sleeve into the 30 × 20 × 15 brick (outer brick).
Figure 9. Solution B step-by-step execution process: (a) pre-drilling of the bricks with a 5 mm drill; (b) drilling of the bricks with a 14 mm drill; (c) placement of the closed-end sock sleeve into the 30 × 20 × 11 brick (inner brick); (d) filling of the sock sleeve with the cement based grout; (e) placement of the helical tie rod into the hole and the outer brick sock sleeve; (f) sock sleeve into the 30 × 20 × 15 brick (outer brick).
Buildings 11 00028 g009
Figure 10. Pull-out tests of Solution A: (a) single brick specimens; (b) comparison for pre-existent brick wallette and single brick specimens; (c) comparison for new brick wallette and single brick specimens.
Figure 10. Pull-out tests of Solution A: (a) single brick specimens; (b) comparison for pre-existent brick wallette and single brick specimens; (c) comparison for new brick wallette and single brick specimens.
Buildings 11 00028 g010
Figure 11. Relationship between pull-out force of single specimens and bricks’ compressive strength: (a) brick format 30 × 20 × 11; (b) brick format 30 × 20 × 15.
Figure 11. Relationship between pull-out force of single specimens and bricks’ compressive strength: (a) brick format 30 × 20 × 11; (b) brick format 30 × 20 × 15.
Buildings 11 00028 g011
Figure 12. Pull-out tests of Solution B: (a) single brick specimens; (b) comparison for pre-existent brick wallette and single specimens; (c) comparison for new brick wallette and single specimens.
Figure 12. Pull-out tests of Solution B: (a) single brick specimens; (b) comparison for pre-existent brick wallette and single specimens; (c) comparison for new brick wallette and single specimens.
Buildings 11 00028 g012aBuildings 11 00028 g012b
Figure 13. Relationship between pull-out force of single specimens and bricks’ compressive strength: (a) brick format 30 × 20 × 11; (b) brick format 30 × 20 × 15.
Figure 13. Relationship between pull-out force of single specimens and bricks’ compressive strength: (a) brick format 30 × 20 × 11; (b) brick format 30 × 20 × 15.
Buildings 11 00028 g013
Figure 14. Types of failure observed: (a) fragile; (b) tie-bar slippage; (c) global.
Figure 14. Types of failure observed: (a) fragile; (b) tie-bar slippage; (c) global.
Buildings 11 00028 g014
Figure 15. Test components: (a) hydraulic jack of 300 kN coupled to a load cell of 25 kN; (b) steel grip coupled to the load cell; (c) pull-out test apparatus; (d) full apparatus view.
Figure 15. Test components: (a) hydraulic jack of 300 kN coupled to a load cell of 25 kN; (b) steel grip coupled to the load cell; (c) pull-out test apparatus; (d) full apparatus view.
Buildings 11 00028 g015aBuildings 11 00028 g015b
Table 1. Comparative analysis between Solution A and Solution B: features and benefits.
Table 1. Comparative analysis between Solution A and Solution B: features and benefits.
Solution ASolution B
Features• Safe, quick and easy application;
• Purely mechanical system (frictional resistance), do not requires the use of resins, grouts or mechanical expansion;
• Efficient with the use of bricks, blocks, concrete, hard mortar and wood;
• Efficient in cavity and solid walls, as well as hollowed and perforated materials;
• Can be applied independently of the external environment and/or temperature.
• The capacity to fix the thin layer of the double leaf wall can be easily tested;
• Effective in all constructive materials;
• Excellent connection between tie and plaster;
• Curing time mandatory for cementitious grout.
Benefits• Low acquisition and installation cost;
• High tensile resistance;
• Flexible, able to absorb the natural movement of the structure;
• Can be placed through the insulation system without affecting significantly its thermal efficiency;
• Does not affect the external aspect of the masonry wall;
• Low disturbance for the buildings’ function and occupants.
• Efficient relation between cost and benefit, as well as performance;
• Able to absorb natural building movements;
• Efficient for the rehabilitation of tall buildings;
• Does not affects the buildings’ external appearance;
• Does not disturb the buildings’ occupants.
Table 2. Average compressive strength values.
Table 2. Average compressive strength values.
Type of BrickAverage Compressive Strength (MPa)Coefficient of Variation (%)
30 × 20 × 15 (Post-NP EN 771-1)3.0113
30 × 20 × 15 (Pre-NP EN 771-1)3.7926
30 × 20 × 11 (Post-NP EN 771-1)1.7214
30 × 20 × 11 (Pre-NP EN 771-1)2.7011
Table 3. Pull-out test results of the three groups of new brick specimens.
Table 3. Pull-out test results of the three groups of new brick specimens.
New Brick Specimens
Buildings 11 00028 i001Obs.: Failure by slipping of the tie in the brick 30 × 20 × 11 sock sleeve and slipping of the tie in the brick 30 × 20 × 15 sock sleeve
Dy: 1.65 mm; Du: 34.84 mm; μ: 21.12; fmax.: 2.42 kN
Slipping after yielding: 33.70 mm
In this group of tested specimens it was obtained, on average, a value of 2.7 kN for the maximum pull-out force and 11.74 for ductility.
The abrupt decrease in strength represents the initiation of the tie slippage in the sleeve, leading to the global failure.
Buildings 11 00028 i002Obs.: Global failure
Dy: 2.61 mm; Du: 28.32 mm; μ: 10.85; fmax: 2.02 kN
Slipping after yielding: 24.7 mm
For the second group of specimens, the average value obtained for the pull-out force was 1.9 kN and a ductility of 10.78 was also obtained.
In general, the grout bulbs formed did not possess flaws (cracks, irregularities), showing a regular and consistent formation.
Buildings 11 00028 i003Obs.: Brittle failure
Dy: 1.84 mm; Du: 7.08 mm; μ: 3.85; fmax: 1.29 kN
Slipping after yielding: 4.16 mm
The third group of isolated specimens of new bricks obtained an average value of 2.14 kN for the pull-out force and 3.11 for ductility.
When the maximum pull-out force and yielding occurs is reached, the specimen no longer has capacity to attain pull-out strength values near this maximum.
Legend: Dy: displacement obtained in the maximum peak of strength; Du: displacement obtained before the rupture; μ: ductility; fmax: maximum pull-out force.
Table 4. Pull-out test results of the two groups of pre-existent brick specimens.
Table 4. Pull-out test results of the two groups of pre-existent brick specimens.
Pre-Existent Brick Specimens
Buildings 11 00028 i004Obs.: Sliding of the tie in the sleeve for both bricks
Dy: 1.65 mm; Du: 42.02 mm; μ: 25.47; fmax: 3.10 kN
Slipping after yielding: 40.37 mm
This group of tested specimens obtained an average value of 2.93 kN for the pull-out force and 12.74 for ductility.
After the rupture, it was observed that certain sock sleeves were damaged, which corroborates the fact that there was slippage of the ties.
Buildings 11 00028 i005Obs.: Brittle failure for the brick 30 × 20 × 11 and slipping of the sock sleeve in the brick 30 × 20 × 15.
Dy: 1.49 mm; Du: 17.29 mm; μ: 11.60; fmax: 1.67 kN
Slipping after yielding: 15.80 mm
In this second group, it was obtained, on average, a value of 2.90 kN for the pull-out force and 12.99 for ductility.
Highlight that, firstly, a rupture of the first web was noticed, with an abrupt loss of strength. Then the second web of the brick was solicited; however, the maximum strength attained is 50% lower when compared with the maximum value obtained.
Legend: Dy: displacement obtained in the maximum peak of strength; Du: displacement obtained before the rupture; μ: ductility; fmax: maximum pull-out force.
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Rebelo, F.; Figueiredo, A.; Correia Lopes, G.; Ferreira, T.M.; Vicente, R. Development of Retrofitting Solutions: Remedial Wall Ties for Masonry Enclosure Brick Walls. Buildings 2021, 11, 28. https://doi.org/10.3390/buildings11010028

AMA Style

Rebelo F, Figueiredo A, Correia Lopes G, Ferreira TM, Vicente R. Development of Retrofitting Solutions: Remedial Wall Ties for Masonry Enclosure Brick Walls. Buildings. 2021; 11(1):28. https://doi.org/10.3390/buildings11010028

Chicago/Turabian Style

Rebelo, Filipe, António Figueiredo, Gonçalo Correia Lopes, Tiago Miguel Ferreira, and Romeu Vicente. 2021. "Development of Retrofitting Solutions: Remedial Wall Ties for Masonry Enclosure Brick Walls" Buildings 11, no. 1: 28. https://doi.org/10.3390/buildings11010028

APA Style

Rebelo, F., Figueiredo, A., Correia Lopes, G., Ferreira, T. M., & Vicente, R. (2021). Development of Retrofitting Solutions: Remedial Wall Ties for Masonry Enclosure Brick Walls. Buildings, 11(1), 28. https://doi.org/10.3390/buildings11010028

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop