Article

Boron Nitride Nanotubes Versus Carbon Nanotubes: A Thermal Stability and Oxidation Behavior Study

by
Nikolaos Kostoglou
1,*,
Christos Tampaxis
2,
Georgia Charalambopoulou
2,
Georgios Constantinides
3,
Vladislav Ryzhkov
4,
Charalabos Doumanidis
5,
Branko Matovic
6,
Christian Mitterer
1 and
Claus Rebholz
1,7
1
Department of Materials Science, Montanuniversität Leoben, 8700 Leoben, Austria
2
National Center for Scientific Research Demokritos, 15341 Athens, Greece
3
Department of Mechanical and Materials Science and Engineering, Cyprus University of Technology, 3036 Lemesos, Cyprus
4
Research School of High-Energy Physics, Tomsk Polytechnic University, 634050 Tomsk, Russia
5
College of Engineering and Computer Science, VinUniversity, Hanoi 100000, Vietnam
6
Vinča Institute of Nuclear Sciences, University of Belgrade, 11000 Belgrade, Serbia
7
Department of Mechanical and Manufacturing Engineering, University of Cyprus, 1678 Nicosia, Cyprus
*
Author to whom correspondence should be addressed.
Nanomaterials 2020, 10(12), 2435; https://doi.org/10.3390/nano10122435
Submission received: 16 October 2020 / Revised: 27 November 2020 / Accepted: 3 December 2020 / Published: 5 December 2020

Abstract

:
Nanotubes made of boron nitride (BN) and carbon have attracted considerable attention within the literature due to their unique mechanical, electrical and thermal properties. In this work, BN and carbon nanotubes, exhibiting high purity (>99%) and similar surface areas (~200 m2/g), were systematically investigated for their thermal stability and oxidation behavior by combining thermal gravimetric analysis and differential scanning calorimetry methods at temperatures of up to ~1300 °C under a synthetic air flow environment. The BN nanotubes showed a good resistance to oxidation up to ~900 °C and fully transformed to boron oxide up to ~1100 °C, while the carbon nanotubes were stable up to ~450 °C and almost completely combusted up to ~800 °C. The different oxidation mechanisms are attributed to the different chemical nature of the two types of nanotubes.

1. Introduction

Nanostructured materials have been a “hot” research topic in recent years since improved properties are expected compared to their bulk phase counterparts [1,2]. In this respect, one-dimensional tubular structures with nano-sized diameters, widely known as nanotubes, have attracted significant attention over the past three decades. Carbon nanotubes (CNTs) and boron nitride nanotubes (BNNTs), the most well-known nanotubular representatives, share the same crystal structure (i.e., sp2-bonded atoms forming hexagonal rings), even though they are composed of different elements [3,4]. However, the C-C bond is purely covalent while the B-N bond is partially ionic due to the difference in electronegativity between B and N elements [5]. Although CNTs and BNNTs exhibit similar properties (e.g., tensile strength, Young’s modulus, thermal conductivity), they also demonstrate profound differences (e.g., CNTs are metallic or semiconducting while BNNTs are electrically insulating) [6]. Both types of nanotubes have been considered for a series of emerging applications, even for controlled and targeted drug delivery [7,8]
Despite their remarkable properties, BNNTs have received far less attention than CNTs within the literature. More specifically, a detailed search on the Scopus database for peer-reviewed publications on BNNTs and CNTs between the years 2000 and 2019 revealed a distinct difference in their total number (see Figure 1). Characteristically, only ~200 papers related to BNNTs were published in 2019 in contrast to ~15,900 papers referring to CNTs (i.e., ratio of ~1:80), as seen in Figure 1a. Furthermore, the cumulative number of publications on BNNTs hardly reached 1600 (in the period 2000–2019), while the respective ones on CNTs exceeded 100,000 (see Figure 1b). Such a characteristic difference can be attributed to the greater difficulty in the production of BNNTs and by consequence to the limited availability of BNNTs over the time [9].
A key property of BNNTs, also substantially different compared to CNTs, is related to their superior high-temperature resistance, even in atmospheric conditions, which opens new pathways for emerging applications (e.g., aerospace industry) where robust materials are required to withstand extreme conditions [10]. In this context, it has been suggested that crystallinity, particle shape and size, specific surface area (SSA), and purity play a significant role in the thermal stability and oxidation behavior of BN materials [11,12,13]. More specifically, crystalline BN materials with large particle size or small SSA seem to provide less reactive sites favorable for oxidation. We have previously investigated highly crystalline and pure (>98%) BN nanoplatelets with a low SSA (~23 m2/g) [14], as well as porous and highly pure (>99%) BN nanoplatelets with a larger SSA (~213 m2/g) [13] and reported oxidation resistance temperatures of up to ~1000 °C and ~800 °C, respectively. Taking into consideration that most of the previous studies found in the literature, focusing on the comparison of laboratory-synthesized BNNTs and CNTs, have shown a lack of high-purity nanotubes (i.e., a significant amount of catalytic remnants can influence the oxidation behavior) and/or have not considered the SSA values of these materials (i.e., lack of reports on gas sorption data), the comparison of the high-temperature properties of high-purity BNNTs and CNTs with similar SSA values is clearly of fundamental interest.
The current study presents a systematic investigation and comparison of the high-temperature properties of two isostructural materials (BNNTs and CNTs) of high purity that demonstrate different chemistry but similar crystallinity and SSA. The respective oxidation mechanisms are highlighted for each case and the influence of the chemical nature is discussed. Properties related to morphology, microstructure, surface chemistry, and porosity were deduced using scanning electron microscopy (SEM), transmission electron microscopy (TEM), X-ray diffraction (XRD), Fourier-transform infrared spectroscopy (FT-IR), and N2 adsorption/desorption measurements at −196 °C. The thermal stability and oxidation behavior were examined by combining thermal gravimetric analysis (TGA) and differential scanning calorimetry (DSC) under synthetic air-flow conditions.

2. Materials and Methods

Multi-walled BNNTs were obtained from BNNT LLC Company (Newport News, VA, USA) and were produced by a high temperature-pressure method, also known as pressurized vapor condenser method [10]. Multi-walled CNTs were acquired from Chengdu Organic Chemicals Company Ltd. Chinese Academy of Sciences (Chengdu, China) and were synthesized by chemical vapor deposition via decomposition of natural gas over a Ni-based catalyst followed by chemical purification using a mixture of potassium permanganate and sulfuric acid.
SEM images were collected by a FEI Quanta 200 microscope (Hillsboro, OR, USA) using a 20 kV acceleration voltage and a working distance of 10 mm. Prior to SEM analysis, the samples were sputter-coated with Au with the aim to improve their conductivity and avoid potential charging effects during imaging. For an alternative and rapid assessment of the surface area to volume ratio, fractal dimension analysis of the SEM images was performed by box-counting algorithms of four different measures (capacity, information, correlation, and probability) using the FDim image processing software [15]. TEM micrographs were recorded by a Philips CM-20 microscope (Eindhoven, Netherlands) with high-resolution capabilities equipped with a LaB6 filament using a 200 kV acceleration voltage. The samples were ultra-sonicated in ethanol and were placed onto holey carbon-only support films mounted on copper grids. A statistical analysis of the outer and inner diameters for both types of nanotubes was carried out by measuring 150 nanotubes (for each case) from low and high-magnification TEM images.
X-ray diffractograms were collected by a Bruker-AXS D8 Advance diffractometer (Karlsruhe, Germany) equipped with CuKα radiation (λ ~ 0.154 nm) at 40 kV voltage and 40 mA current. The XRD measurements were performed using a continuous scan speed mode in the diffraction angle range 2θ = 10–60°, a 0.01° step width and a 0.5 °/min scan speed in Bragg–Brentano geometry. The interlayer distances were calculated from the (002) reflections using Bragg’s law, while the crystallite thicknesses and crystallite lateral sizes were estimated from the (100)/(101) reflections using Scherrer formula. FT-IR spectra were recorded by a JASCO-4100 spectrometer (Shangai, China) in the mid-infrared region between 4400 and 400 cm−1. Samples of ~1 mg were prepared in a pellet form by using potassium bromide.
N2 adsorption/desorption isotherms were collected at −196 °C using a Quantachrome Autosorb-1-MP gas sorption analyzer (Boynton Beach, FL, USA) and ultra-pure (99.999%) N2. Before the measurements, samples of ~50 mg were degassed under high vacuum (10−6 mbar) at 250 °C for 24 h. The Brunauer–Emmet–Teller (BET) area values were calculated following the pertinent consistency criteria (ISO 9277:2010).
TGA and DSC curves were simultaneously recorded by a SETARAM SETSYS Evolution-18 thermal analyzer (Caluire, France) in the temperature range 25–1300 °C using a 10 °C/min heating rate and a 16 mL/min synthetic air flow. Samples of ~10 mg were placed in alumina crucibles, while buoyancy effects were taken into consideration by performing a blank measurement. Prior to thermal analysis, purging was applied to remove residual contamination from inside the furnace.

3. Results and Discussion

3.1. Surface Morphology

Figure 2a–f display SEM images at different magnifications for the BNNTs and CNTs. The BNNTs consist of nanotube bundles held together in a ‘web-like’ structure (see Figure 2a–c), while the CNTs exhibit a ‘spaghetti-like’ morphology (see Figure 2d–f). Both materials present a typical multi-walled nanotubular structure, as evidenced from the high-resolution TEM images (see Figure 3). Open-ended nanotubes can be mostly observed in the case of CNTs (see Figure 3c,d), which is most likely attributed to the chemical purification process that followed their production. The BNNTs seem to exhibit a slightly smaller outer and inner diameter (7.6 ± 2.8 nm and 3.1 ± 1.3 nm, respectively) compared to the CNTs (12.3 ± 4.3 nm and 5.0 ± 1.6 nm, respectively), as determined by low- and high-magnification TEM images. More information about the statistical analysis in the nanotube diameters can be found in the box plots of Figure 4. The average values of the fractal dimension parameters, measured with four different algorithms, showed only a 4% difference between the two materials (see Table 1), thus suggesting comparable surface area-to-volume ratios.

3.2. Microstructure and Surface Chemistry

The XRD and FT-IR analysis for the BNNTs and CNTs are presented in Figure 5. The X-ray diffractograms (see Figure 5a) indicated very similar structural characteristics for the two materials. The BNNTs pattern shows features related to the hexagonal BN structure (JCPDS card no. 34-0421), including the (002), (100)/(101), and (004) reflections at 2θ ~25.6°, ~42.3°, and ~53.1°, respectively. Similarly, the graphitic (002) reflection at 2θ ~25.9° is dominating the CNTs pattern (JCPDS card no. 75-1621), followed by the less-pronounced (100)/(101) and (004) reflections at ~42.8° and ~53.5°, respectively. The CNTs pattern is slightly shifted to higher 2θ angles, thus indicating slightly narrower interlayer spacing. The interlayer distances for BNNTs and CNTs were estimated at ~0.348 and ~0.344 nm, respectively, which are larger than those of hexagonal BN (0.330–0.333 nm) and graphite (0.333–0.335 nm) [16]. The average crystallite thicknesses and crystallite lateral sizes were estimated around 3 nm and 12 nm, respectively, for both materials. No other peaks related to impurities were detected in both cases, which confirms the high purity of these materials in terms of BN and carbon, respectively. Similar XRD patterns for high-purity BNNTs and CNTs have been reported in recent studies [17,18].
The FT-IR spectra (see Figure 5b) revealed distinctively different surface chemistries for the two materials. The BNNTs exhibit characteristic bands at ~795 and ~1377 cm−1, attributed to the out-of-plane B–N–B bending and the in-plane B–N stretching vibration modes, respectively [19]. Less-intensive and broader bands around ~2365 and ~3400 cm−1 are due to atmospheric CO2 and adsorbed H2O, respectively. In contrast, the CNTs spectrum is almost featureless with a low signal-to-noise ratio due to intense absorption of infrared radiation from the carbon. Weak and broad bands shown in the 1000–1700 cm−1 region are probably due to the C–O/C=O vibrations of oxygen-based functionalities (e.g., carboxyls) and the C=C stretching vibration mode of sp2 carbon [20]. The CO2 band is also visible in this case. The carbon nature of the CNTs was also confirmed by Raman spectroscopy, where typical disorder-induced and graphitic bands were observed (see Figure S1 in Supplementary Materials).

3.3. Porosity and Surface Area

Both materials demonstrated a comparable N2 adsorption/desorption behavior at −196 °C (see Figure 6a), thus suggesting a similar pore structure. The main difference is the slightly increased adsorbed N2 volume of the CNTs both at lower (i.e., P/P0 < 0.1; see Figure 6a inset) and higher (i.e., P/P0 ~ 0.99) relative pressures. The small hysteresis loop formed between the adsorption and the desorption curves at P/P0 > 0.85 is attributed to capillary condensation of N2 in mesopores (i.e., pore widths 2–50 nm) [21]. The sudden rise of the adsorption curve at P/P0 ~ 0.99 and the lack of a saturation “plateau” describe condensation of N2 in macropores (i.e., pore widths larger than 50 nm) or N2 adsorption onto external surfaces [22]. The calculated BET areas (see Figure 6b) showed only a ~10% difference, i.e., ~180 and ~198 m2/g for BNNTs and CNTs, respectively.

3.4. Thermal Stability and Oxidation Behavior

TGA and DSC curves under synthetic air (Figure 7) suggested completely different oxidation behaviors for the BNNTs and CNTs. For the BNNTs (Figure 7a), the initial mass decreased by ~4% up to ~150 °C due to desorption of H2O, CO2, and other physisorbed surface contaminations [23]. This can be identified by the weak endothermic DSC peak shown below 150 °C and is much clearer in the differential TGA (dTGA) curve (Figure 7b). Between ~150 and 600 °C, the BNNTs mass remained stable (only decreased by another ~1%) with no pronounced DSC signals, thus indicating the absence of any chemical reactions or phase transformations up to ~600 °C. The decomposition initiated at temperatures beyond 600 °C and the subsequent oxidation was completed at ~1100 °C. The boron reacts with oxygen (O2) from the synthetic air and produces boron trioxide (B2O3), while the nitrogen is released as a molecular gas (N2), based on the chemical reaction 4BN + 3O2 → 2B2O3 + 2N2. Nitric oxide (NOx) gases might be also released during oxidation, as shown previously [24].
In more detail, the BN oxidation can be distinguished in two regions: (a) initial oxidation between ~600 and 900 °C and (b) active oxidation between ~900 and 1100 °C. For (a), a mass gain of ~10% was observed between ~600 and 900 °C, most probably due to oxidation of external/distorted nanotube layers and B2O3 formation [25]. The DSC and dTGA curves indicated only a broad peak centered around 650 °C. For (b), the TGA curve showed a steeper rise between ~900 and 1100 °C and finally reached a saturation point (mass increased further by ~33%), most likely attributed to oxidation of inner nanotube layers and complete transformation to B2O3 [13]. The strong exothermic DSC peak as well as the fast reaction rate of the dTGA curve (see Figure 7b) in the same range further confirmed the above observations. The oxidation did not proceed beyond 1100 °C and the excess oxidized mass remained stable up to ~1300 °C. It should be noted that the total mass increased by ~43% between ~600 and 1100 °C, which agrees well with the theoretical maximum mass gain of 40.3% by complete BN oxidation into B2O3.
For the CNTs (Figure 7c), the initial mass decreased by ~4% up to ~450 °C. The mass loss below 200 °C is attributed to removal of physisorbed species [26], as indicated by the broad ‘hump’ in the dTGA curve (see Figure 7d). The active oxidation initiated at temperatures beyond 450 °C and an almost complete ‘burnout’ was achieved at ~800 °C (i.e., drastic mass loss by ~95%). The carbon reacts with O2 from the synthetic air and gaseous CO2 is released. Three different oxidation profiles are identified from the exothermic DSC signals at ~550, ~750, and ~800 °C, respectively. Such distinctive oxidation behaviors are related to the diverse reactivity of inner and outer nanotube layers to thermal decomposition [20,26]. The DSC peaks agree well with the dTGA trend in the same temperature range (see Figure 7d). The minor residual mass (~1%), left upon combustion and up to ~900 °C, could be a synthesis remnant (e.g., metal catalyst) used to produce the CNTs.
To sum up, the main difference between the oxidation of BNNTs and CNTs lies in the form of their produced oxides. On the one side, B2O3 forms as a solid deposit right onto the oxidizing nanotube surface, thus retarding the oxidation process of the BNNTs. On the other side, CO2 is a volatile gaseous product, which hardly retards the oxidation process of the CNTs, while carbon oxidation to CO2 also generates defects/holes in the nanotube structure, thus further facilitating the combustion of the CNTs.

4. Conclusions

High-purity (>99%) BNNTs and CNTs, with comparable BET areas (~200 m2/g), were thermally analyzed up to 1300 °C in synthetic air. BNNTs withstood temperatures of up to ~900 °C prior to complete transformation to B2O3 at ~1100 °C, while CNTs remained stable only up to ~450 °C and almost fully ‘burned’ at 800 °C. The different oxidation profiles are explained by the different chemical nature of the nanotubes and the formation of different oxides during combustion.

Supplementary Materials

The following are available online at https://www.mdpi.com/2079-4991/10/12/2435/s1, Figure S1: Raman spectrum for the CNTs.

Author Contributions

Conceptualization, N.K. and C.R.; Methodology, N.K. and C.R.; Validation, N.K. and C.T.; Formal analysis, N.K., V.R., and C.D.; Investigation, N.K., C.T., and G.C. (Georgios Constantinides); Resources, G.C. (Georgia Charalambopoulou), C.M., and C.R.; Data curation, N.K., V.R., and C.D.; Writing—original draft preparation, N.K. and C.R.; Writing—review and editing, G.C. (Georgia Charalambopoulou), G.C. (Georgios Constantinides), V.R., C.D., B.M., and C.M.; Visualization, N.K. and C.R.; Supervision, C.M. and C.R.; Project administration, N.K. and C.R. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding. The APC was funded by the University of Cyprus.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Kolahalam, L.A.; Kasi Viswanath, I.V.; Diwakar, B.S.; Govindh, B.; Reddy, V.; Murthy, Y.L.N. Review on nanomaterials: Synthesis and applications. Mater. Today Proc. 2019, 18, 2182–2190. [Google Scholar] [CrossRef]
  2. Prakash Sharma, V.; Sharma, U.; Chattopadhyay, M.; Shukla, V.N. Advance Applications of Nanomaterials: A Review. Mater. Today Proc. 2018, 5, 6376–6380. [Google Scholar] [CrossRef]
  3. Iijima, S. Helical microtubules of graphitic carbon. Nature 1991, 354, 56–58. [Google Scholar] [CrossRef]
  4. Chopra, N.G.; Luyken, R.J.; Cherrey, K.; Crespi, V.H.; Cohen, M.L.; Louie, S.G.; Zettl, A. Boron nitride nanotubes. Science 1995, 269, 966–967. [Google Scholar] [CrossRef]
  5. Cohen, M.L.; Zettl, A. The physics of boron nitride nanotubes. Phys. Today 2010, 63, 34–38. [Google Scholar] [CrossRef] [Green Version]
  6. Kim, J.H.; Pham, T.V.; Hwang, J.H.; Kim, C.S.; Kim, M.J. Boron nitride nanotubes: Synthesis and applications. Nano Converg. 2018, 5, 17. [Google Scholar] [CrossRef] [Green Version]
  7. Wong, B.S.; Yoong, S.L.; Jagusiak, A.; Panczyk, T.; Ho, H.K.; Ang, W.H.; Pastorin, G. Carbon nanotubes for delivery of small molecule drugs. Adv. Drug Deliv. Rev. 2013, 65, 1964–2015. [Google Scholar] [CrossRef]
  8. Ciofani, G. Potential applications of boron nitride nanotubes as drug delivery systems. Expert Opin. Drug Deliv. 2010, 7, 889–893. [Google Scholar] [CrossRef]
  9. Jakubinek, M.B.; Ashrafi, B.; Martinez-Rubi, Y.; Guan, J.; Rahmat, M.; Kim, K.S.; Dénommée, S.; Kingston, C.T.; Simard, B. Boron nitride nanotube composites and applications. In Nanotube Superfiber Materials: Science, Manufacturing, Commercialization; Elsevier: Amsterdam, The Netherlands, 2019; pp. 91–111. ISBN 9780128126677. [Google Scholar]
  10. Tiano, A.L.; Park, C.; Lee, J.W.; Luong, H.H.; Gibbons, L.J.; Chu, S.-H.; Applin, S.; Gnoffo, P.; Lowther, S.; Kim, H.J.; et al. Boron nitride nanotube: Synthesis and applications. In Nanosensors, Biosensors, and Info-Tech Sensors and Systems 2014; Varadan, V.K., Ed.; SPIE: Bellingham, WA, USA, 2014; Volume 9060, p. 906006. [Google Scholar]
  11. Hou, X.; Yu, Z.; Li, Y.; Chou, K.C. Preparation and properties of hexagonal boron nitride fibers used as high temperature membrane filter. Mater. Res. Bull. 2014, 49, 39–43. [Google Scholar] [CrossRef]
  12. Wang, L.; Hang, R.; Xu, Y.; Guo, C.; Qian, Y. From ultrathin nanosheets, triangular plates to nanocrystals with exposed (102) facets, a morphology and phase transformation of sp2 hybrid BN nanomaterials. RSC Adv. 2014, 4, 14233–14240. [Google Scholar] [CrossRef]
  13. Kostoglou, N.; Lukovic, J.; Babic, B.; Matovic, B.; Photiou, D.; Constantinides, G.; Polychronopoulou, K.; Ryzhkov, V.; Grossmann, B.; Mitterer, C.; et al. Few-step synthesis, thermal purification and structural characterization of porous boron nitride nanoplatelets. Mater. Des. 2016. [Google Scholar] [CrossRef]
  14. Kostoglou, N.; Polychronopoulou, K.; Rebholz, C. Thermal and chemical stability of hexagonal boron nitride (h-BN) nanoplatelets. Vacuum 2015, 112, 42–45. [Google Scholar] [CrossRef]
  15. Falconer, K.J. Fractal Geometry: Mathematical Foundations and Applications; Wiley: Hoboken, NJ, USA, 2003; ISBN 0470871350. [Google Scholar]
  16. Hod, O. Graphite and hexagonal boron-nitride have the same interlayer distance. Why? J. Chem. Theory Comput. 2012, 8, 1360–1369. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  17. Amin, M.S.; Atwater, B.; Pike, R.D.; Williamson, K.E.; Kranbuehl, D.E.; Schniepp, H.C. High-purity boron nitride nanotubes via high-yield hydrocarbon solvent processing. Chem. Mater. 2019, 31, 8351–8357. [Google Scholar] [CrossRef]
  18. Hammadi, A.H.; Jasim, A.M.; Abdulrazzak, F.H.; Al-Sammarraie, A.M.A.; Cherifi, Y.; Boukherroub, R.; Hussein, F.H. Purification for Carbon Nanotubes Synthesized by Flame Fragments Deposition via Hydrogen Peroxide and Acetone. Materials 2020, 13, 2342. [Google Scholar] [CrossRef]
  19. Harrison, H.; Lamb, J.T.; Nowlin, K.S.; Guenthner, A.J.; Ghiassi, K.B.; Kelkar, A.D.; Alston, J.R. Quantification of hexagonal boron nitride impurities in boron nitride nanotubes: Via FTIR spectroscopy. Nanoscale Adv. 2019, 1, 1693–1701. [Google Scholar] [CrossRef] [Green Version]
  20. Lehman, J.H.; Terrones, M.; Mansfield, E.; Hurst, K.E.; Meunier, V. Evaluating the characteristics of multiwall carbon nanotubes. Carbon N. Y. 2011, 49, 2581–2602. [Google Scholar] [CrossRef]
  21. Thommes, M.; Kaneko, K.; Neimark, A.V.; Olivier, J.P.; Rodriguez-Reinoso, F.; Rouquerol, J.; Sing, K.S.W. Physisorption of gases, with special reference to the evaluation of surface area and pore size distribution (IUPAC Technical Report). Pure Appl. Chem. 2015, 87, 1051–1069. [Google Scholar] [CrossRef] [Green Version]
  22. Kostoglou, N.; Ryzhkov, V.; Walters, I.; Doumanidis, C.; Rebholz, C.; Mitterer, C. Arc-produced short-length multi-walled carbon nanotubes as “millstones” for the preparation of graphene-like nanoplatelets. Carbon N. Y. 2019, 146, 779–784. [Google Scholar] [CrossRef]
  23. Chen, Y.; Zou, J.; Campbell, S.J.; Caer, G. Le Boron nitride nanotubes: Pronounced resistance to oxidation. Appl. Phys. Lett. 2004, 84, 2430–2432. [Google Scholar] [CrossRef] [Green Version]
  24. Lavrenko, V.A.; Alexeev, A.F. High-temperature oxidation of boron nitride. Ceram. Int. 1986, 12, 25–31. [Google Scholar] [CrossRef]
  25. Nautiyal, P.; Loganathan, A.; Agrawal, R.; Boesl, B.; Wang, C.; Agarwal, A. Oxidative Unzipping and Transformation of High Aspect Ratio Boron Nitride Nanotubes into “white Graphene Oxide” Platelets. Sci. Rep. 2016, 6, 1–8. [Google Scholar] [CrossRef] [PubMed]
  26. Likodimos, V.; Steriotis, T.A.; Papageorgiou, S.K.; Romanos, G.E.; Marques, R.R.N.; Rocha, R.P.; Faria, J.L.; Pereira, M.F.R.; Figueiredo, J.L.; Silva, A.M.T.; et al. Controlled surface functionalization of multiwall carbon nanotubes by HNO3 hydrothermal oxidation. Carbon N. Y. 2014, 69, 311–326. [Google Scholar] [CrossRef]
Figure 1. Search results in Scopus (September 2020) for (a) the annual number of peer-reviewed publications on BNNTs and CNTs (the solid bars for BNNTs can be barely noticed) and (b) the cumulative number of peer-reviewed publications between the years 2000 and 2019.
Figure 1. Search results in Scopus (September 2020) for (a) the annual number of peer-reviewed publications on BNNTs and CNTs (the solid bars for BNNTs can be barely noticed) and (b) the cumulative number of peer-reviewed publications between the years 2000 and 2019.
Nanomaterials 10 02435 g001
Figure 2. SEM images at different magnifications for (ac) BNNTs and (df) CNTs.
Figure 2. SEM images at different magnifications for (ac) BNNTs and (df) CNTs.
Nanomaterials 10 02435 g002
Figure 3. TEM images at different magnifications for (a,b) BNNTs and (c,d) CNTs.
Figure 3. TEM images at different magnifications for (a,b) BNNTs and (c,d) CNTs.
Nanomaterials 10 02435 g003
Figure 4. Box plots for the outer and inner nanotube diameters of the BNNTs and CNTs as measured by low- and high-magnification TEM images; the circle marker and the bold line correspond to the mean and median values, respectively.
Figure 4. Box plots for the outer and inner nanotube diameters of the BNNTs and CNTs as measured by low- and high-magnification TEM images; the circle marker and the bold line correspond to the mean and median values, respectively.
Nanomaterials 10 02435 g004
Figure 5. (a) X-ray diffractograms and (b) FT-IR spectra for the BNNTs and CNTs.
Figure 5. (a) X-ray diffractograms and (b) FT-IR spectra for the BNNTs and CNTs.
Nanomaterials 10 02435 g005
Figure 6. (a) N2 adsorption (solid symbols) and desorption (open symbols) isotherms recorded at −196 °C for the BNNTs and CNTs; the inset shows the N2 adsorption behavior at the lower relative pressures (P/P0 < 10−1) using a logarithmic scale and (b) linear multi-point BET plots calculated at the relative pressure range 0.06 < P/P0 < 0.22.
Figure 6. (a) N2 adsorption (solid symbols) and desorption (open symbols) isotherms recorded at −196 °C for the BNNTs and CNTs; the inset shows the N2 adsorption behavior at the lower relative pressures (P/P0 < 10−1) using a logarithmic scale and (b) linear multi-point BET plots calculated at the relative pressure range 0.06 < P/P0 < 0.22.
Nanomaterials 10 02435 g006
Figure 7. (a) Combined TGA/DSC and TGA/dTGA curves in synthetic air for (a,b) BNNTs and (c,d) CNTs; dTGA stands for differential TGA (temporal mass change).
Figure 7. (a) Combined TGA/DSC and TGA/dTGA curves in synthetic air for (a,b) BNNTs and (c,d) CNTs; dTGA stands for differential TGA (temporal mass change).
Nanomaterials 10 02435 g007
Table 1. Fractal dimension parameters deduced from SEM images (Figure 2).
Table 1. Fractal dimension parameters deduced from SEM images (Figure 2).
MaterialSEM ImageCapacityInformationCorrelationProbability
BNNTsFigure 2a2.512.402.172.36
BNNTsFigure 2b2.532.402.162.30
BNNTsFigure 2c2.392.252.122.30
CNTsFigure 2d2.552.432.192.46
CNTsFigure 2e2.492.382.192.39
CNTsFigure 2f2.302.182.092.26
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Kostoglou, N.; Tampaxis, C.; Charalambopoulou, G.; Constantinides, G.; Ryzhkov, V.; Doumanidis, C.; Matovic, B.; Mitterer, C.; Rebholz, C. Boron Nitride Nanotubes Versus Carbon Nanotubes: A Thermal Stability and Oxidation Behavior Study. Nanomaterials 2020, 10, 2435. https://doi.org/10.3390/nano10122435

AMA Style

Kostoglou N, Tampaxis C, Charalambopoulou G, Constantinides G, Ryzhkov V, Doumanidis C, Matovic B, Mitterer C, Rebholz C. Boron Nitride Nanotubes Versus Carbon Nanotubes: A Thermal Stability and Oxidation Behavior Study. Nanomaterials. 2020; 10(12):2435. https://doi.org/10.3390/nano10122435

Chicago/Turabian Style

Kostoglou, Nikolaos, Christos Tampaxis, Georgia Charalambopoulou, Georgios Constantinides, Vladislav Ryzhkov, Charalabos Doumanidis, Branko Matovic, Christian Mitterer, and Claus Rebholz. 2020. "Boron Nitride Nanotubes Versus Carbon Nanotubes: A Thermal Stability and Oxidation Behavior Study" Nanomaterials 10, no. 12: 2435. https://doi.org/10.3390/nano10122435

APA Style

Kostoglou, N., Tampaxis, C., Charalambopoulou, G., Constantinides, G., Ryzhkov, V., Doumanidis, C., Matovic, B., Mitterer, C., & Rebholz, C. (2020). Boron Nitride Nanotubes Versus Carbon Nanotubes: A Thermal Stability and Oxidation Behavior Study. Nanomaterials, 10(12), 2435. https://doi.org/10.3390/nano10122435

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop