1. Introduction
Mucormycosis is an angio-invasive fungal infection that is caused by saprophytic fungi belonging to the order
Mucorales. Infection is associated with complications that are characterized by tissue necrosis and infarction of blood vessels [
1,
2,
3]. A comparison of global data on mucormycosis indicates that the case burden of mucormycosis was estimated to be 70 times higher in India during the COVID-19 pandemic [
4,
5]. A multi-country study on COVID-19-associated mucormycosis (CAM) reported that 53% of the cases were from India, followed by the United States of America (10%), Pakistan (6.3%), France (5%), Mexico (5%), Iran (5%), and Russia (2.5%) [
6]. During the second wave associated with the COVID-19 pandemic, the caseload of mucormycosis increased drastically (>50,000 cases) in India, prompting the Indian health authorities to declare mucormycosis as an endemic disease [
7]. The situation is challenging due to the limited availability of first-line antifungal drugs, such as liposomal amphotericin and amphotericin B deoxycholate. Because of the high abundance of clinically relevant
Mucorales in Indian soils, sporangiospores are highly prevalent in indoor and outdoor air [
2,
8]. Patients acquire the infection by inhalation, ingestion, or traumatic inoculation of the viable sporangiospores from the environment. Morphologically, the
Mucorales sporangiospores (especially
R. arrhizus sporangiospores) are ~2–5 μm in size; the sporangiospore wall exhibits a rough, amorphous outer surface and a fibrillar inner surface. Structurally, the spore wall can be composed of three layers: (a) an outer characteristic electron-opaque layer with a thickness of 10–240 nm, sometimes covered by a fragile extra layer, (b) an electron-dense ~160–245 nm thick layer, and (c) an innermost layer of relatively high electron density covering the plasma membrane (~15–40 nm thick). Chemically, the major spore wall components are proteins, glucan, chitosan, and melanin, followed by smaller amounts of uronic acids, lipids, chitin, and mannose. The protein(s) contain high aspartic acid and glutamic acid levels, followed by glycine, alanine, lysine, histidine, and serine, and smaller amounts of other amino acids.
The antifungal activity of silver nanoparticles is well documented in various fungal species; however, the metal nanoparticle-mediated sporicidal activity of
Mucorales member
R. arrhizus is underreported to this point. Silver cations are considered a Lewis acid, which reacts with a Lewis base; Lewis bases include phosphorous and sulfur-containing biomolecules, which are found in significant components of the cell wall, cell membrane, proteins, and DNA bases [
9]. Mechanistically, silver nanoparticles can cover the cell surface through non-specific interaction with biomolecules on the cell wall and membrane, leading to morphological changes, such as shrinkage of the cytoplasm, membrane detachment, and the formation of numerous electron-dense pits, which ultimately cause cell death [
10,
11,
12]. A hydrophilic, cationic polymer coating on silver nanoparticles may allow for the selective interaction of silver nanoparticles with the microbial cell; as such, enhanced antifungal activity can be observed. Incorporating a cationic charge on nanoparticles and other types of inorganic materials entails surface modification with cationic polymers (e.g., poly-amidoamine, poly-ethyleneimine (PEI), and poly-lysine) via covalent or electrostatic mechanisms and surface grafting with amine groups [
13,
14,
15]. In addition, in the process of nanoparticle formation, the size may further be controlled as a function of molecular weight (
Mw) and the working concentration of the polymer. In our present study, we have assessed the germination inhibition and anti-sporangiospores activity of PEI-functionalized Ag-NPs as a function of PEI molecular weight (
Mw 700,000 Da and 65,000 Da), which modulated surface charge and size of silver nanoparticles, against clinically isolated
R. arrhizus.
2. Materials and Methods
2.1. Materials
The polyethyleneimine (PEI), silver nitrate, and propidium iodide (PI) were obtained from Sigma-Aldrich (Bangalore, Karnataka, India). Fungal culture media, such as RPMI (Roswell Park Memorial Institute, Buffalo, NY, USA), Sabouraud dextrose agar (SDA), and broth, were collected from Hi-Media Laboratories Ltd. (Mumbai, Maharashtra, India). Plasticware was purchased from Tarsons Products Private Ltd. (Kolkata, West Bengal, India). Amphotericin B and other routine chemicals were purchased from Sigma-Aldrich (St. Louis, MO, USA). Finally, solvents were purchased from Merck Life Science Private Limited (Bangalore, Karnataka, India). All the reagents were of analytical grade.
2.2. Fungal Strain
This study was approved by the Institution Ethical Committee, Institute of Medical Sciences, at Banaras Hindu University, Varanasi (Dean/2021/EC/3003, dated 29 October 2021). Here, we used a clinical strain of R. arrhizus isolated from a 46-years-old male suffering from rhino-orbital mucormycosis during the second wave of the SARS-CoV2 infection in India. The strain was identified as per standard mycological procedure, including culture and morphological characteristics. For further experiments, the isolated strain was sub-cultured in SD broth and preserved in 25% glycerol at −80 °C.
2.3. Harvesting of Sporangiospores
The preserved culture was sub-cultured on a Sabouraud dextrose agar slant for 4–6 days at 30 °C, and the sporangiospores of
R. arrhizus were harvested as per the method of Singh et al. 2011. [
16] In brief, a total of 10 mL of 0.9% saline solution was then added to the slant tube, followed by repeated washing of the mycelia with the added saline. The resulting suspension was collected and centrifuged at 3500×
g for 8 min; the pellet was washed with 0.1 M PBS and resuspended in 0.9% saline. The spores were counted using a Neubauer hemacytometer, and the counts were expressed as sporangiospores/mL.
2.4. Synthesis and Physical Characterization of PEI Functionalized Silver Nanoparticles
The PEI functionalized silver nanoparticles (PEI-f-AgNP-1 and 2) were synthesized as described previously by Tiwari et al. 2020 with a slight modification [
17]. In short, 120 µL of ethylene glycol and a methanolic 1-vinyl 2-pyrrolidone solution (50 µL of a 250 mM solution) were placed in 2 mL glass vial, followed by the inclusion of a methanolic AgNO
3 solution (20 µL of a 10 mM solution), PEI 1 (
Mw 700,000) and 2 (
Mw 65,000) (50 and 25 µL of a 20 mg/mL solution, respectively, in separate vials), and cyclohexanone (20 μL). The reaction mixture was thoroughly mixed using a vortex mixer for 30 s and then placed in a microwave oven for 10 s. The cycle was repeated 4–6 times in a microwave oven, leading to the formation of a deep yellow color that signified the formation of PEI-f-Ag-NP-1 and 2. The synthesized silver nanoparticles were dispersible in water without any physical changes. All the experiments were conducted with a dilution of silver nanoparticles in ultrapure water.
All the polyethyleneimine functionalized silver nanoparticles (PEI-f-Ag-NPs) were characterized using a U-2900 UV-Vis spectrophotometer (Hitachi, Tokyo, Japan) over the scan range of 250–800 nm. Selected area electron diffraction and transmission electron microscopy analysis of Ag-NPs were carried out using a Tecnai G20 Twin instrument (FEI, Hillsboro, OR, USA). Samples were prepared by diluting the Ag-NPs in methanol and drop-casting the solution on carbon-coated copper grids of 300 mesh. Zeta potential analysis was performed using a Zetasizer instrument (Malvern Panalytical, Malvern, UK). All graphs were plotted on Origin 2018 software (OriginLab Corporation, Northampton, MA, USA).
2.5. Assessment of In Vitro Antifungal Activity of Silver Nanoparticles
The 4–6 day grown culture on SD agar of isolated
R. arrhizus was prepared and the sporangiospores were harvested, as described previously. The harvested sporangiospores were washed with PBS twice, resuspended in RPMI liquid medium, and adjusted to 2 × 10
7 spores per mL in a 5 mL test suspension. 50 µg (100 µL of stock solution) of synthesized silver nanoparticles (PEI-f-AgNP-1 and 2) were inoculated in each test suspension. Similarly, amphotericin B (2 µg/mL) was taken as the positive control, and a distilled water inoculated suspension was taken as the negative control. All the test samples were incubated at 28 °C for 72 h. To assess the sporangiospore morphology after treatment with PEI-f-Ag-NP-1 and 2, a 10 µL of treated aliquot was obtained at various time intervals (24, 48, and 72 h) from each tube, placed on a glass slide, covered with glass slip, and observed under a bright-field binocular compound light microscope (Olympus, Tokyo, Japan) with 40× objective lenses. The anti-sporangiospore activity was confirmed by inoculating 5 µL of treated aliquots on SD agar plates. All the tests were repeated in triplicate, and average values were determined. The spore diameter of the ungerminated (freshly harvested), germinated (negative control), and PEI-f-Ag-NPs treated samples was measured using the following formula:
The spore diameter was calculated with the help of ImageJ software (NIH, Bethesda, MD, USA), and the values were plotted using Origin 8.5 2018 software (OriginLab Corporation, Northampton, MA, USA) to create statistical histograms.
2.6. Minimum Inhibitory Concentration (MIC) Determination of PEI-f-Ag-NPs
The MIC data for PEI-functionalized silver nanoparticles (PEI-f-AgNP-1 and 2) against R. arrhizus sporangiospores (0.5–5 × 104 spores/mL) were obtained using the two-fold serial dilution method in a flat-bottom sterile 96-well microtiter plate. An active suspension of 50 µg/mL PEI-f-Ag-NPs was prepared; 100 µL of each suspension was distributed in the wells using the double dilution approach; the final concentration was between 0.10 and 50 µg/mL. Subsequently, 100 µL of the sporangiospore suspension was added to each well. Amphotericin B and sterile distilled water were used as a positive control and negative control, respectively. The microtiter plate was incubated in a static position at 28 °C for 72 h; visual demonstration of turbidity (i.e., a visually clear well) was recorded as the MIC. After that, a 10 µL aliquot from each well was sub-cultured on the SD agar plates for 72 h; fungal growth was subsequently observed. The MIC data were determined as the concentration of PEI-f-Ag-NPs at which the growth was inhibited or slowed compared to the standard control.
2.7. Studies on Germination Attenuation of Sporangiospores
R. arrhizus sporangiospores were prepared, as described previously [
16]. The spore germination inhibition assay was performed, as described previously [
18]. Briefly, 100 µL of sporangiospore suspensions (10
7 spores/mL) were mixed with PEI-f-Ag-NP 1 and 2 in the separate tubes with a final concentration of 0.41, 0.82, 1.65, and 3.30 μg/mL for PEI-f-AgNP-1 and 1.62, 3.25, 6.50, and 13.0 µg/mL for PEI-f-AgNP-2. Control samples (positive and negative) contained sporangiospores suspensions with 50 µL (0.50 µg/mL) of amphotericin B and 50 µL of distilled water, respectively. The 50 µL mixture with a different concentration of PEI-f-Ag-NPs was transferred onto a sterile concave slide for incubation at 28 °C. Three slides were prepared for each treatment, and mean values were compared. A hundred sporangiospores per treatment were observed at an interval of 24 h for germination inhibition of sporangiospores using a bright-field binocular compound light microscope (Olympus, Tokyo, Japan). The spore germination rate was calculated as follows [
18]:
2.8. Cell Morphology Observation with Scanning Electron Microscopy (SEM)
The ultrastructural changes in PEI-f-AgNP-1 and 2 treated sporangiospores were investigated using SEM. Initially, the sporangiospore suspensions were treated with PEI-f-Ag-NP-1 and 2 for 24 h at 28 °C, followed by centrifugation at 3500 rpm for 6 min. The condensed cells were fixed with 2.5% glutaraldehyde and postfixed with 1% aqueous OsO4, followed by washing with 0.1 M (pH 7.0) phosphate buffers. Subsequently, the samples were dehydrated in an ascending concentration of ethanol in a serial manner at 30, 50, 70, 80, 90, and 100% for 15 min and dried in a vacuum oven. Finally, the cells were placed on the glass coverslip, coated with gold, and observed using a JSM-6700F SEM (JEOL, Tokyo, Japan).
2.9. Confocal Laser Scanning Microscopy (CLSM) Studies
Confocal microscopic examination was performed to assess the viability of sporangiospores incubated with PEI-f-Ag-NP-1 and 2 [
18]. Briefly, 5 mL of freshly prepared sporangiospore suspensions (2 × 10
7 spores/mL) was prepared as described above, and treated with 50 µL of PEI-f-Ag-NP 1 and 2 each at its MIC value in a separate tube along with positive and negative controls (amphotericin B and distilled water) at 28 °C for 72 h. A 1 mL of aliquot was withdrawn every 24 h interval from each tube and centrifuged at 3500 rpm for 5 min. The pellet was washed twice with PBS (0.1 M) and resuspended in PBS. The spores were stained with 10 µL (1 mg/mL stock) of propidium iodide (PI) (excitation/emission at 535 nm/617 nm) for 25 min in the dark and washed again to eliminate excess dye with PBS (phosphate buffer saline). Subsequently, the treated samples were observed under an SP5 AOBS confocal lesser scanning microscope (Leica, Wetzlar, Germany) with a 40× immersion oil objective. The anti-sporangiospore activity of PEI-f-Ag-NP-1 and 2 were confirmed by the fact that dead (damaged cell membrane) sporangiospores stain with propidium iodide and live spores remained unstained since intact plasma membrane prevents the passage of potassium iodide (PI) inside the cell.
2.10. Surface Enhanced Raman Spectroscopy (SERS) Studies
For the confocal Raman spectroscopic study, the PEI-f-Ag-NP-1 and 2 treated and untreated sporangiospores suspensions were centrifuged at 3500 rpm for 6 min. The semi-solid suspension was spotted on a cover glass and dried under ambient conditions. Confocal Raman measurements were obtained using a CRM Alpha 300 S instrument (WiTec GmbH, Ulm, Germany). The excitation source for this study was a 532 nm Nd: YAG laser, and the maximum power output of the laser was 40 mW. The laser power was attenuated to ≈10 mW to the sampling point. Measurements were performed using a 100× objective. The dispersed light intensity of the signal from the grating was measured by a Peltier-cooled charge-coupled device (CCD). The maximum area of laser exposure was 750 nm, and the collection was performed confocally. Spectra were collected in the 400–2100 cm
−1 window [
19]. The band peaks were matched with respective wavenumber values from the work of Joke De Gelder et al. [
20].
4. Discussion
Mucormycosis is a life-threatening infection caused by R. arrhizus, a saprophytic fungus, which commonly occurs in diabetic and hematopoietic stem cell transplant patients. During the second wave of COVID-19 (March–June 2021) in India, ~51,775 mucormycosis cases were reported, for which uncontrolled hyperglycemia was considered the most common predisposing risk factor. The free-floating environmental sporangiospores enter the human body through inhalation, where they primarily colonize and infect the paranasal sinuses, nasal cavity, and orbit. In this study, we have investigated the anti-sporangiospore activity and impact of polyethyleneimine functionalized silver nanoparticles on the germination of sporangiospores and their antifungal mechanism.
Polyethyleneimine is a polycationic, hydrophilic polymer, which is used for DNA transfection of mammalian cells, drug delivery, and material coatings in the biomedical and industrial fields. We have documented the synthesis of polyethyleneimine functionalized silver nanoparticles in previous studies [
17]. Apart from polyethyleneimine, other biocompatible silica-containing organic polymers, such as organotrialkoxysilane (e.g., 3-aminopropyltrimethoxysilane and 3-glycidoxytrimethoxysilane), along with organic reducing agents cyclohexanone and formaldehyde, are being used for the controlled synthesis of monometallic, bimetallic, and trimetallic noble metal nanoparticles [
22]. During the synthesis of NPs, we used methanol and an organic monomer, 1-vinyl 2 pyrrolinone, to reduce the silver cation reactivity with PEI and protect the synthesized nanoparticles from agglomeration. Subsequently, synthesized PEI-f-Ag-NPs were reconstituted in ultra-pure HPLC-grade water to determine their anti-sporangiospore activity.
The synthesized PEI-f-Ag-NPs showed UV-Vis absorption maxima at 420 and 408 nm, respectively (
Figure 1A). The molecular weight of polyethyleneimine affects the size of silver nanoparticles, which resulted in this shifting; the size was confirmed by TEM (
Figure 1B). It was interesting to observe that the higher molecular weight PEI (
Mw 700,000 Da) led to the synthesis of larger-sized PEI-f-AgNP-1 (~20.4 ± 5.9 nm); in comparison, the PEI-f-AgNP-2 synthesized with lower molecular weight PEI (65,000 Da) had a size of ~4.2 ± 0.7 nm. Apart from the molecular weight variation, the PEI concentration also controls the size of synthesized NPs; this relationship was evident from UV-Vis spectrophotometry (as reported previously) [
17,
31]. The molecular weight of PEI depends on the number (n) of monomers, which, proportionately, increases the net cationic charge of the molecule. The ζ value of both PEI-f-Ag-NPs was positive because of the greater number of amine groups exposed on the PEI surface [
31]. Therefore, the ζ potential of synthesized PEI-f-Ag-NPs depends on the molecular weight of PEI (
Figure 2). However, Ortega et al. reported on the mechanism of PEI functionalized silver nanoparticles in detail and suggested that the PEI-mediated redox reaction promotes nucleation and growth of NPs, resulting in the formation of size-dependent particles [
31]. Initially, the silver cation (Ag
+) forms a complex with non-bonding electrons (nitrogen atoms) of the PEI amine group. Such bonding leads to the nucleation and growth of NPs. To promote the complete redox reaction, a microwave oven was used to yield stable NPs. However, the role of molecular weight of PEI in the size determination of NPs has not been fully elucidated and requires a more detailed investigation.
We used a clinical strain of
R. arrhizus, which was isolated from a patient suffering from COVID-19-associated mucormycosis, to explore sporangiospore survival and germination behavior in the presence of the synthesized PEI-f-Ag-NPs. Both PEI-f-AgNP-1 and 2 showed significant anti-sporangiospore activity and attenuated germination within 24 h of exposure. During incubation of sporangiospores with PEI-f-AgNP-1, we observed an interesting behavior in which a few populations of sporangiospores were swollen (~14 μm in size) much larger as compared to the control with increasing time. Usually, the swollen sporangiospores result from water absorption before germ tube formation [
23,
24]. PEI-f-AgNP-1 exposure resulted in the killing of most of the sporangiospores; a few remained alive, which failed to germinate, despite having altered size and shape (
Figure 3 and
Figure 4a,b).
In contrast, PEI-f-AgNP-2-treated sporangiospores did not show any abnormal behavior as most of the cells were fractured. This difference in the anti-sporangiospore activity of the PEI-f-Ag-NPs is due to differences in the cationic surface charge as a function of the molecular weight of PEI. Although the results followed the MIC of both PEI-f-Ag-NPs, PEI-f-AgNP-1 had a lower MIC (1.65 μg/mL) than PEI-f-AgNP-2 (6.5 μg/mL). Despite having a higher MIC, PEI-f-AgNP-2 showed a significant detrimental impact on the cytoarchitecture of
R. arrhizus sporangiospores. This finding can be explained by the difference in the charge and size of the PEI-f-Ag-NPs. PEI-f-AgNP-1 is larger in size and highly cationic (~20.4 nm ± 5.9, charge +25 mV). It usually fails to enter the sporangiospores (compared to PEI-f-AgNP-2); however, this large size NPs probably undergoes frequent collisions and forms strong electrostatic interaction with sporangiospores (
Figure 5a).
Further, the anti-sporangiospore activity of both PEI-f-Ag-NPs was confirmed by a confocal laser scanning microscopy study that involved staining of the sporangiospores with PI dye. The PI fluorophore binds with cellular DNA and fluoresces red when illuminated at a specific wavelength of light (488/617 nm). The PI molecule cannot cross the intact cell membrane; however, an altered cell membrane allows for cytoplasmic entry. The CLSM study confirmed cell membrane damage within 24 h of incubation with PEI-f-Ag-NPs (
Figure 6a). After incubation (e.g., at 48 and 72 h), DNA compaction and fragmentation were observed more commonly in PEI-f-AgNP-2-treated sporangiospores, indicating the internalization of PEI-f-AgNP-2 (
Figure 6b,c). It has been reported that highly charged PEI molecules interact more strongly with the cell surface than less cationic charged molecules since a tight electrostatic interaction forms between negatively charged cell surfaces.
Interestingly, the PEI-f-AgNP-2 had a small and low cationic surface charge; it likely entered the cells and caused nucleic acid damage. On the other hand, reactive oxygen species (ROS) generated by PEI-f-AgNP-2 resulted in an alteration of cell membrane permeability with subsequent nucleic acid damage. However, PEI-f-AgNP-1 altered the cell membrane permeability due to strong electrostatic interaction-induced ROS generation. Further, we observed that sporangiospores not exposed to PEI-f-Ag-NPs also had PI staining after 24 h of incubation. This phenomenon is considered an effect of increased water absorption, resulting in increased cell membrane permeability to the dye [
23].
Further, to observe the ultrastructural changes in PEI-f-Ag-NPs treated sporangiospores, SEM-EDS was performed (
Figure 7). We observed that PEI-f-AgNP-1-treated sporangiospores had a smooth surface without characteristic longitudinal ridges. This finding is probably due to the collapse of membrane potential with subsequent cytoplasmic substance leakage because of strong electrostatic interaction-mediated ROS generation, which further indicates the lack of cellular internalization of PEI-f-AgNP-1 (
Figure 7b). In contrast, the smaller PEI-f-AgNP-2 with low cationic surface charge showed cell fracture as observed in SEM-EDS, which supported the light microscopy and CLSM imaging observations. Cell fracture may be attributed to indirect internalization of PEI-f-AgNP-2 via proton channels or porins or direct penetration of the cell wall and membrane, inducing the ROS generation and cytoarchitectural damage (
Figure 7c). Similar observations have been confirmed by SEM-EDS analysis of PEI-f-Ag-NPs-treated samples (
Figure 8a–c). Furthermore, SEM-EDS analysis has shown the absence of elemental silver in PEI-f-AgNP-1-treated sporangiospores, which may be due to the washing out of nanoparticles from the sporangiospore surface during sample preparation. In contrast, sporangiospores treated with PEI-f-AgNP-2 contained elemental silver, further indicating the internalization of PEI-f-AgNP-2 nanoparticles within the sporangiospores.
Raman spectroscopy is a non-destructive, rapid technique requiring only small sample volumes, which is associated with nearly no water interference. The bands in Raman spectra are well resolved compared to similar spectroscopic techniques- such as infrared spectroscopy [
30]. De Gussem et al. analyzed
Lactarius spore composition, and Edwards et al. studied lichens using Raman spectroscopy methods [
32,
33]. To understand the interaction of PEI-f-Ag-NPs with sporangiospores, a SERS study was performed on PEI-f-Ag-NPs-treated sporangiospores and germinated mycelium; freshly harvested sporangiospores served as a control (
Figure 9). The results confirmed cell wall/membrane damage and cytoplasmic leakage by PEI-f-Ag-NPs. Among the fingerprint biomolecules, few common metabolites and nucleotides were identified in the treated sporangiospores (e.g., trehalose (407 cm
−1), cytosine (537, 582 cm
−1), thymine (617 cm
−1), ꞵ-carotene (1008 cm
−1), acetyl CoA (1243 cm
−1), and amylopectin (1264 cm
−1)). The presence of glutathione and trehalose in PEI-f-AgNP-1-treated sporangiospores indicated nanoparticle-induced ROS generation [
34,
35]. Trehalose is a nonreducing sugar-containing two glucose subunits with an α, α-1,1-glycosidic linkage [
36]. In fungi, trehalose is present in all structures of the life cycle, such as spores, fruiting bodies, vegetative cells, and hyphae, which rapidly deplete after germination. In addition, trehalose serves a role in central fungal metabolism and in responses to specific environmental stress. Trehalose forms hydrogen bonds with surrounding water molecules and functions as a replacement for water by interacting with phospholipids or other macromolecules in the cell membrane under stress conditions [
36]. This study identified trehalose in freshly harvested and PEI-f-Ag-NPs-treated sporangiospores at 407 cm
−1. However, it was also present in the germinated mycelial control at 1455 cm
−1, which indicated molecular changes, such as bond stretching or bending (
Figure 9). The identification of cellular metabolites, such as acetyl coenzyme A and ꞵ- carotene, indicated the presence of a damaged cell wall/membrane in treated sporangiospores. In
Mucorales, ꞵ- carotene synthesizes sporopollenin polymers, protecting sporangiospores in a stressful environment. N-acetylglucosamine, detected in PEI-f-AgNP-1-treated sporangiospores at 1126 cm
−1, is the cell wall component of bacteria and fungi; it was reported previously in yeast cells via SERS spectroscopy at 1125 cm
−1 [
34]. Thus, shifts in the Raman spectra of N-acetylglucosamine have been assigned to stretching in CO and CC bonds and out-of-plane bending in CH bonds, suggesting sporangiospores wall damage. Further, a D-galactosamine peak was observed in both PEI-f-Ag-NPs-treated sporangiospores at 462 cm
−1; however, it was absent in the mycelial and sporangiospore control samples, indicating surface structural deformations. In addition, we also observed considerable biomolecular differences between freshly harvested sporangiospores and fully germinated sporangiospores mycelia. Very few biomolecules identified in germinated mycelia (e.g., glycerol (416 cm
−1), succinic acid (582 cm
−1), 14 methylpentadecanoic acid (814 cm
−1), and triolein (1065 cm
−1)). The Raman signal in treated and control samples was somewhat low and needed more process optimization for the analysis of molecular changes, such as bond stretching and bending in molecules. However, a detailed study is under way.
Possible Anti-Sporangiospores Mechanism of PEI-f-Ag-NPs
Our previous study reported that PEI functionalized silver nanoparticles as a function of their molecular weight interacted with the surface-expressed proteins of
Acinetobacter bauminnii and quenched their autofluorescence [
17,
37]. However, in our present study, the anti-sporangiospore mechanism on
R. arrhizus indicates a different pathway. The PEI functionalized silver nanoparticles (PEI-f-AgNP-1 and 2) differed in their size and zeta potential, as discussed above, as a function of the molecular weight of PEI. Due to the variable physical properties of PEI-f-Ag-NPs, the mode of action against the sporangiospores may be different. As our findings discussed above, it is plausible that PEI-f-AgNP-1 interacts electrostatically at the nano-bio interface with negatively charged sporangiospores, resulting in stress-induced ROS generation that leads to the inactivation of biomolecules with subsequent swelling and cellular leakage. In contrast to PEI-f-AgNP-1, PEI-f-AgNP-2 had a smaller size and low zeta potential and, as such, may enter the cell directly as a nanoparticle bullet or indirectly through proton channel/porins. The proposed model is shown in
Figure 10.