Next Article in Journal
Thermally Reduced Graphene Oxide/Carbon Nanotube Composite Films for Thermal Packaging Applications
Next Article in Special Issue
Methodology for Revealing the Phases and Microstructural Constituents of the CMSX-4 Nickel-Based Superalloy Implicating Their Computer-Aided Detection for Image Analysis
Previous Article in Journal
Influence of the Titanium Implant Surface Treatment on the Surface Roughness and Chemical Composition
Previous Article in Special Issue
Parametric Formulae for Elastic Stress Concentration Factor at the Weld Toe of Distorted Butt-Welded Joints
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Strengthening of AA5754 Aluminum Alloy by DRECE Process Followed by Annealing Response Investigation

1
Division of Material Processing Technology, Management and Computer Techniques in Materials Science, Institute of Engineering Materials and Biomaterials, Silesian University of Technology, 44-100 Gliwice, Poland
2
Department of Mechanical Technology, Faculty of Mechanical Engineering, VŠB-Technical University of Ostrava, 17. listopadu 15, 708 33 Ostrava, Czech Republic
3
Research Centre of University of Zilina, University of Zilina, 010 26 Zilina, Slovak Republic
4
Paks’D Sp z.o.o. Strzelecka 74, 43-100 Tychy, Poland
*
Author to whom correspondence should be addressed.
Materials 2020, 13(2), 301; https://doi.org/10.3390/ma13020301
Submission received: 3 December 2019 / Revised: 3 January 2020 / Accepted: 6 January 2020 / Published: 10 January 2020
(This article belongs to the Special Issue Structure and Mechanical Properties of Alloys)

Abstract

:
In this study, a dual rolls equal channel extrusion (DRECE) process has been applied for improving the mechanical properties of the 5754 alloy. Supplementary experiments involving metallography, electron backscattered diffraction (EBSD), and XRD tests were carried out to evaluate the effect of the DRECE process. XRD analysis showed that the maximum dislocation density was achieved after six DRECE passes, which were accompanied by the formation that is typical for low-strain structures. The increasing dislocation density, as well as grain refinement throughout DRECE deformation, resulted in an increase in the mechanical properties. Annealing of the as-deformed sample resulted in grain growth and strength reduction.
Keywords:
DRECE; XRD; EBSD; structure

1. Introduction

Severe plastic deformation (SPD) processes are regarded as appropriate for the manufacturing of bulk samples having a nano or ultrafine-grained microstructure via imposing significant plastic strain (which is difficult to obtain using the conventional deformation technique). Several different SPD processing methods are now available i.e., HPT (high-pressure torsion), TE (twist extrusion), or ARB (accumulative roll bonding) [1,2,3]. However, in recent years, the ECAP (equal channel angular pressing) method attracted the greatest interest. In this procedure, the workpiece, in the form of a rod or bar having a circular cross-section, is pressed through a die that consists of two channels that meet at a predetermined angle: usually 90 degrees [4]. A significant limitation of conventional ECAP is the size of the work samples and process discontinuity. The work sample must be repeatedly reinserted in the die channel for several consecutive passes to impose high strain. This type of procedure from a practical point of view has a disadvantage of high labor input requirement during the deformation process, and it may be used easily only for fundamental laboratory investigations. The ECAP process is discontinuous and slow, which makes it impractical in industrial applications. Due to that, critical attention has been focused on the possibility of alternative processing procedures development that is continuous and precludes the need for removing and reinserting the work samples after every deformation cycle. Several attempts have been made to enhance the effectiveness of the SPD processes. For instance, continuous cyclic bending [5], repetitive corrugation and straightening (RCS) [6], accumulative roll bonding [7], ECAP conform [8], or dual rolls equal channel extrusion (DRECE) [9] have been used successfully to produce fine-grained microstructures on a large scale.
The DRECE method is a modification/combination of two commonly known SPD techniques: the DCAP method (dissimilar channel angular pressing) and ECAP-CONFORM (continuous equal-channel angular pressing), and it has been developed for forming metal sheets with maximum dimensions of 1000 × 60 × 2 mm. In this technique, the sample is inserted into the working space and then extruded through the roller without changing their dimension. The critical factor that influences the mechanical properties of the material after the DRECE process is a proper selection of the output geometry in the deformation zone–deformation angle (123°, 118° or 108°) [10]. When comparing the DRECE method to the other commonly known SPD techniques, we must remember that the strain accumulation after a single pass is not as high as i.e., in the ECAP process. Similar to the ECAP process, the repetitive deformations increase the accumulated strain, which affects the microstructure and thus changes the mechanical properties. The main advantage of the DRECE method is the length of the work specimen and the form of the batch material sheet. Such form of the batch material is typical i.e., for automotive industry applications.
The 5754 aluminum alloy used in this study is typically supplied to automotive manufacturers, where it is used for car body parts and door structural components. This is because of its unique properties, including moderate strength, high corrosion resistance, weldability, and easy forming characteristics [11]. These properties can be increased by severe plastic deformation processes by employing the grain refinement process [12,13]. However, conventional SPD processes provide only laboratory-scale samples, which cannot be applied industrially. Therefore, in this investigation, we focused on the DRECE method and its possible application to enhance the mechanical properties of the 5754 aluminum–magnesium alloy.

2. Materials and Methods

The investigated material was an aluminum–magnesium alloy 5754 that had the chemical composition given in Table 1.
The DRECE process with the principle is shown in Figure 1 was conducted at VŠB-Technical University in Ostrava in the Department of Mechanical Engineering. In this experiment, we set the deformation α angle to be 108°.
The 5754 alloy samples covered with a Gleit grease were subjected up to six DRECE passes without changing the sample orientation between subsequent passes. The pressure of the feed roller was set to 150 bar. The sample was processed with a constant deformation speed of 40 mm/min. To investigate the thermal stability of the obtained microstructure, the sample was subjected to isothermal annealing at 150 °C, 180 °C, 200 °C, 250 °C, 300 °C, and 350 °C respectively for 30 min after six DRECE passes.
The microstructures were examined using a light microscope Axio Observer Z1. To reveal the grain size and morphology, the samples were mechanically ground and polished and then electrolytically etched using Barker’s reagent.
To study the microstructural evolution in a greater detail, the 5754 aluminum alloy samples were twin-jet electropolished in an electrolyte containing 20% nitric acid and 80% methanol at a temperature of −30 °C and 20 V for 15 s. Then, the grain structure was recorded by orientation imaging microscopy (OIM) using the electron backscattered diffraction (EBSD) technique integrated with a Zeiss Supra 35 Scanning Electron Microscope controlled and analyzed using OIM software (EDAX, Inc., Mahwah, NJ, USA). An area 60 × 60 μm was scanned on the normal direction plane, and the step size was taken to be 0.2 μm in all scans. A neighbor orientation correlation data cleaning process (level 4), followed by a grain confidence index (CI) standarization cleanup with a grain tolerance angle threshold set to 2°, was used. After the data cleaning, a coincidence index filter of 0.05 was used to remove the points that were not indexed correctly.
X-ray diffraction analysis was carried out on the electropolished sections of the samples by employing a PANalytical X’Pert Pro diffraction system (Malvern Panalytical Ltd., Royston, UK) equipped with a CuKα radiation source, 30 kV, and 30 mA with a scan rate of 0.005°/s. The average crystallite size was calculated from the four Bragg reflection peaks of fcc-Al: (111), (200), (220), and (311) using the Scherrer and Wilson equation [14].
D v = 0.9 λ B c o s θ B
where Dv is the effective crystallite size, λ is the X-ray wavelength, θ is the Bragg angle, and B is the line broadening. The microstrain was calculated using the Williamson Hall equation [15].
B c o s θ = 0.9 λ D v + 4 ε s i n θ
where ε is the root mean square of microstrain. According to the Rietveld method, the dislocation density can be estimated from the following equations:
ρ = ρ d · ρ s 1 / 2
ρ d = 3 / D v 2
ρ s = ε 2 / b 2
where ρd and ρs are the dislocation density due to domains and the dislocation density due to the microstructure, respectively.
Finally, the microhardness (HV) of the specimens were measured along the thickness by a microhardness tester Future-Tech FM-ARS under a load of 300 g for 15 s. Tensile tests were carried out using Zwick Z100 equipment (ZwickRoell GmbH & Co.KG, Ulm, Germany) with a strain rate of 6.7 × 10−4 s−1.

3. Results and Discussion

3.1. Initial Microstructure

Figure 2 is an optical micrograph of 5754 alloy in an unprocessed state. This figure shows a typical wrought microstructure built of equiaxed grains. According to Cabibbo [16], the 5754 alloy matrix consist of a Mg in Al solid solution with fine dispersoids of Mg2Si and Al6Mn phases.

3.2. Effect of DRECE on Dislocation Density

Figure 3 shows the X-ray diffraction profiles of 5754 alloy samples in a different condition. As shown, the main reflections for the fcc Al (111), (200), (220), (311), and (400) were detected. In addition, two supplementary peaks at 2θ = 40.21° and 58.11 were identified to be characteristic of the Mg2Si phase. The diffraction peaks of the as-deformed samples are broadened, and their intensities change throughout the DRECE process. According to Ungar [17], this can be due to an increased amount of dislocations accumulated during severe plastic deformation and the small size of the diffracting grains Additionally, the peak shift expresses that the DRECE process causes a substantial amount of distortion in the lattice structure of Al5754 alloy. This can be related to long range stresses generated by severe plastic deformation.
The summarized results of the structural parameters obtained from XRD analysis are presented in Table 2. Throughout DRECE processing, the average domain size parameter decreased from ~35 nm in an initial state to ~29 nm after six DRECE passes. In addition, after DRECE processing, the dislocation density increased from 3.46 × 1014 m−2 in the unprocessed state to 6.47 × 1014 m−2 after the first pass. Then, the dislocation density showed a steady decrease with an increasing number of passes, indicating the annihilation of dislocations despite increased strain accumulation [18], reaching a saturation level of 7.55 × 1014 m−2 after six DRECE passes. This result is in accordance with the results of other works for similar Al–Mg alloys. Dinkerl [19] has documented that the dislocation density of AlMg2 alloy was calculated by XRD to be ~5 × 1014 m−2~3 × 1014 m−2 and 12 ECAP passes, respectively. According to Liu [20], the dislocation density of an AA5182 alloy after five turns of the HPT process increased to 12.8 × 1014 m−2.

3.3. Evolution of Microstructure

Figure 4a–f shows an optical micrograph (longitudinal plane) of 5754 aluminum alloy subjected up to six DRECE passes. As compared with the initial state of the microstructure (Figure 2), the grain size is not reduced significantly. Areas of different crystallographic orientations inside individual grains are visible. For the micrographs shown, it appears that the increase in the number of DRECE passes is not accompanied by noticeable changes in the microstructure. Throughout subsequent passes, the grains remain equiaxed and almost constant in size.
Figure 5 shows the EBSD colored inverse pole figure (IPF) maps of the 5754 aluminum alloy samples in an initial state and subjected to one, four, or six DRECE passes, respectively. In these microstructures, the grain color/shade corresponds to the individual grain orientation denoted by the unit triangle legend in Figure 5b. The red lines indicate the locations of high-angle grain boundaries (θ >15°), while green lines indicate the locations of low-angle grain boundaries (3°> θ >15°). The IPF image of the initial state sample (Figure 5a) demonstrates that the microstructure is composed of equiaxed grains. The measured average intercept length prior deformation is ~7.916 μm. Figure 5b shows the microstructure after the first DRECE pass. According to the unit triangle legend used, several orientations can be observed even in the grain interiors. This indicates the variation in crystal orientation in the grain interiors at the early stages of deformation. The average intercept length remains almost unchanged: ~7.862 μm. Figure 5c shows the effect of four DRECE passes. In this condition, the grain interiors are covered with many elongated bands of cells, having a low-angle grain boundary misorientation. These deformation bands are almost parallel to the TD direction. The measured average intercept length decreased to ~6.872 μm. Figure 5d shows the microstructure of the sample subjected to six DRECE passes. In this state, the microstructure consists of grains covered with deformation bands having a low angle misorientation. This type of microstructure is typical for aluminum alloys subjected to low strains [21,22]. The measured average intercept length after six DRECE passes slightly increases to ~6.958 μm.
Detailed extracted values of the fraction of the grain boundaries are presented in Figure 6 and Table 3. In the initial state, the fraction of HAGBs is very high ~88.4% and slightly decreases after the first DRECE pass to ~86.6%. Along with the increase in the number of deformation passes, the fraction of HAGBs decreases. After four DRECE passes, approximately 58.6% of the grains have a grain boundary misorientation of more than 15°, indicating HAG (high-angled grains). Finally, the opposite trend is visible. After six DRECE passes, the fraction of HAGBs (high-angle grain boundaries) slightly increases to 59.6%.

3.4. Mechanical Properties after DRECE Process

Figure 7 presents the indentation Vickers microhardness for an initial state and DRECE processed 5754 alloy samples taken across the thickness of the samples. Additionally, a summary of mechanical properties as a function of DRECE passes is given in Table 4. The observed high hardness gradient between the surface and center of the initial state sample is due to the inhomogeneity of deformation during rolling. The measured mean microhardness value is ~79 Hv. The hardness of the sheet increases throughout DRECE deformation. After the first DRECE pass, this value raises to about ~92 Hv. In addition, in this state, the hardness gradient between the surface and center increases—the hardness values lie in the range of 82–111 Hv. The observed hardness increase is accompanied by a dislocation density growth, as presented in Table 2. Along with increasing strain accumulation, the hardness values slightly increase, reaching a maximal value of ~99 Hv after six passes. It is worth mentioning that the hardness gradient between the surface and center of the samples decreases throughout DRECE deformation—the hardness values lie in the range of 92–108 Hv, indicating that the non-homogeneous hardness distribution (non-uniform deformation) in the as-rolled initial sample remains in the DRECE processed samples. This may be attributed to the nature of the rolling process, in which the imposed strain is higher near the surface, while a lower amount of deformation is applied at the center.
The mechanical properties of 5754 alloy after the DRECE process were also tested in a tensile test at room temperature, as shown in Table 4. It is clear that both yield and tensile strength increase throughout DRECE deformation. For the initial state, the mean yield strength value is 112.3, and this value increases rapidly to 184.7 MPa after the first pass. Then, it rises slightly to 198.2 MPa after six passes. This means that the work-hardening rate reduces with the strain increase. However, the observed strength improvement, which was lower than that with the ECAP method [23,24], was achieved at the expense of ductility, which decreased from 30.1% to about 13.2% after the first DRECE pass; then with an increase in strain accumulation, it decreased to 8.4% after the six DRECE passes. Such changes in strength and ductility are typical for severely deformed metals, as proved in numerous research papers [4,16,25,26].

3.5. Annealing Response of the As-Deformed 5745 Alloy

After the DRECE deformation, a thermodynamically unstable microstructure containing lattice defects and subgrain boundaries was produced. This distorted microstructure increased the mechanical properties. To allow further work operation such as shaping, stamping, or forming, the as-deformed alloy must be softened by annealing. The microstructural changes that occur upon annealing are commonly described with reference to recovery processes, the nucleation of new grains, and their growth. The recovery process reduces the stored energy, but it causes only partial mechanical strength reduction, since the dislocation structure is not rearranged into a stable state.
A further microstructural restoration process—recrystallization—may occur in which a new set of defect-free grains nucleate within the as-deformed microstructure. Although the recrystallization removes some amount of stored dislocations, the material still contains a large fraction of grain/subgrain boundaries, which are thermodynamically unstable. Further annealing causes grain growth, which goes along with the formation of new (defect-free) grains in a lower energy configuration.
Light microscopy characterization of the grain microstructure of the 5754 alloy annealed at 150 °C, 180 °C, 200 °C, 250 °C, 300 °C, and 350 °C is shown in Figure 8. It is apparent that during annealing at 150 °C, the process of recovery dominates. This is accompanied by a substantial dislocation density decrease from 7.55 × 1014 m−2 in the as-deformed condition to 4.68 × 1014 m−2, as shown in Table 5. During annealing at 180–300 °C, the entire microstructure undergoes continuous recrystallization followed by grain growth (Figure 8b–e). The first effect of annealing is visible in the sample annealed at 180 °C (Figure 8b). In this condition, small recrystallized grains can be observed in the microstructure. The formation of the new grains is accompanied by a continuous dislocation density decrease to 4.44 × 1014 m−2. The DRECE processed structure changes completely into coarse-grained and is approximately equiaxed with an increase in annealing temperature, obviously, as illustrated in Figure 8e. This is followed by a gradual dislocation density decrease to 2.05 × 1014 m−2. It is worth mentioning that for the sample annealed at 350 °C, the microstructure exhibit characteristics of both uniform coarsening and, in several places, of discontinuous recrystallization (Figure 8f). Thus, the obtained microstructure is bimodal, and the formation of the bimodal microstructure is accompanied by a slight dislocation density growth to 3.18 × 1014 m−2. This is due to the presence of the new annealed microstructure that gives rise to compressive stress fields to the surrounding small-sized grains, resulting in a relatively lattice distortion and enhancing the dislocation density.
Figure 9 shows the X-ray diffraction profiles of the DRECE processed and annealed 5754 alloy samples. As shown, only the main reflections for the fcc Al (111), (200), (220), (311), and (400) and Mg2Si (220) and (400) phases were detected. The diffraction peaks are slightly broadened, and their intensities change depending on the annealing temperature. The intensity and width of the peaks in an XRD pattern can be correlated to the level of residual stresses and dislocation density, which changes after annealing.
The evolution of Vicker’s microhardness of the isothermally annealed 5754 alloy samples is listed in Table 6. The obtained hardness measurements results are in good agreement with the observed microstructure evolution as well as with structural parameters calculated by XRD.
It is evident, as shown in Table 6, that the hardness decreases rapidly from an initial value of ~99.5 HV after six DRECE pass samples to 81.5 HV after 30 min of isothermal annealing at 150 °C. It is due to the ongoing recovery processes and is accompanied by a rapid dislocation density decrease from 7.55 × 1014 m−1 to 4.68 × 1014 m−1. In this condition, the changes in the grain size are almost indistinguishable (Figure 8), and there is no evidence of the recrystallization processes. With an increase in an isothermal annealing temperature up to 180–200 °C, hardness decreases slightly to ~77 HV. This is accompanied by only a slight dislocation density decrease to 4.16 × 1014. In addition, the microstructure looks quite similar—there is still no evidence of the recrystallization process, see Figure 8a–c. The first evidence of the recrystallization and grain growth can be observed in the sample isothermally annealed at 250 °C; see Figure 8d. This phenomenon is accompanied by a dislocation density reduction and hardness decrease to ~61 HV. Annealing at 300 °C causes a more significant grain growth, as shown in Figure 8e, as well as the greatest dislocation density drop to 2.05 × 1014. However, despite the observed microstructural changes, the hardness remains almost unchanged. It should be pointed out that when the material is subjected to isothermal annealing at 350 °C, a slower softening rate is observed. In addition, the obtained microstructure is different: bimodal. This occurs because some grains have a much faster growth rate than others. Such a bimodal microstructure is inhomogeneous and is built of recrystallized and recovered grains and volumes with an unchanged distorted thermodynamically metastable structure; therefore, it combines the effects of the larger grains, which cause softening and the ultrafine grains that increase the mechanical properties.
In general, the difference in softening behavior reported in this study as a function of increasing annealing temperature is in line with competitive recovery–recrystallization kinetics, where a lower isothermal annealing temperature results in a gradual hardness decrease and resembled softening due to recovery, while at higher temperatures where recrystallization processes arise quickly, softening is faster.

4. Conclusions

An investigation was conducted to study the evolution of microstructure and hardness in bulk aluminum 5754 samples processed by DRECE. After DRECE, the samples were subjected to annealing in order to investigate the microstructure and mechanical properties. The main conclusions of this research are summarized below.
The grain boundary maps for the EBSD data revealed that the fraction of low-angle grain boundaries (LAGBs) increases along with an increasing number of DRECE passes. The DRECE process introduces a network of LAGBs, which may transform into HAGBs with further processing, especially if new shear planes will be activated.
The DRECE process increases the hardness of the 5754 aluminum alloy of about 25% after six passes. It is presented also that the yield and tensile strength reached their maximum values of 198 MPa and 251.8 MPa, respectively, after six passes. The increment of the Vickers microhardness as well as tensile and yield strength can be related to increased dislocation density and grain refinement.
The post-DRECE annealing of six passes of 5754 alloy samples at temperatures lower than 180 °C did not affect the microstructure significantly, indicating that recovery dominates. A continuous grain growth occurred at higher annealing temperatures (180–300 °C) due to the continuous recrystallization. A bimodal microstructure having a bimodal dislocation density distribution was obtained through the discontinuous recrystallization at 350 °C.
The hardness measurements of the annealed sample were consistent with the microstructural and XRD study. Grain coarsening led to a stepwise hardness decrease and resembled softening due to recovery before recrystallization. After annealing at the highest temperature (350 °C), the alloy microhardness significantly decreased to a value lower than that of the initial state alloy.

Author Contributions

Conceptualization, P.S.; methodology, O.H., K.G. and S.R.; investigation, K.G., S.R. and P.M.N.; resources, M.B. and T.D.; data curation, T.D.; writing—original draft preparation, P.S.; writing—review and editing, O.H.; supervision, T.T.; funding acquisition, P.S. and S.R. All authors have read and agreed to the published version of the manuscript.

Funding

The results in this publication were obtained as part of the research co-financed by the rector’s grant in the area of scientific research and development works, Silesian University of Technology, 10/010/RGJ19/0273. Work has been done in connection with project Innovative and additive manufacturing technology—new technological solutions for 3D printing of metals and composite materials, reg. no. CZ.02.1.01/0.0/0.0/17_049/0008407 financed by Structural Founds of Europe Union.

Conflicts of Interest

The authors declare no conflict of interest

References

  1. Tański, T.; Snopiński, P.; Borek, W. Strength and structure of AlMg3 alloy after ECAP and post-ECAP processing. Mater. Manuf. Process 2017, 32, 59–70. [Google Scholar] [CrossRef]
  2. Azushima, A.; Kopp, R.; Korhonen, A.; Yang, D.Y.; Micari, F.; Lahoti, G.D.; Groche, P.; Yanagimoto, J.; Tsuji, N.; Rosochowski, A.; et al. Severe plastic deformation (SPD) processes for metals. CIRP Ann. 2008, 57, 16–735. [Google Scholar] [CrossRef]
  3. Segal, V. Review: Modes and processes of severe plastic deformation (SPD). Materials 2018, 11, 1175. [Google Scholar] [CrossRef] [Green Version]
  4. Snopiński, P.; Tański, T.; Matus, K.; Rusz, S. Microstructure, grain refinement and hardness of Al–3%Mg aluminium alloy processed by ECAP with helical die. Arch. Civ. Mech. Eng. 2019, 19, 287–296. [Google Scholar] [CrossRef]
  5. Takayama, Y.; Miura, T.; Kato, H.; Watanabe, H. Microstructural and Textural Evolution by Continuous Cyclic Bending and Annealing in a High Purity Titanium. Mater. Trans. 2004, 45, 2826–2831. [Google Scholar] [CrossRef] [Green Version]
  6. Huang, J.; Zhu, Y.T.; Alexander, D.J.; Liao, X.; Lowe, T.C.; Asaro, R.J. Development of repetitive corrugation and straightening. Mater. Sci. Eng. A 2004, 371, 35–39. [Google Scholar] [CrossRef]
  7. Saito, Y.; Utsunomiya, H.; Tsuji, N.; Sakai, T. Novel ultra-high straining process for bulk materials—development of the accumulative roll-bonding (ARB) process. Acta Mater. 1999, 47, 579–583. [Google Scholar] [CrossRef]
  8. Derakhshan, J.F.; Parsa, M.H.; Jafarian, H.R. Microstructure and mechanical properties variations of pure aluminum subjected to one pass of ECAP-Conform process. Mater. Sci. Eng. A 2019, 747, 120–129. [Google Scholar] [CrossRef]
  9. Rusz, S.; Cizek, L.; Michenka, V.; Dutkiewicz, J.; Salajka, M.; Hilser, O.; Tylsar, S.; Kedron, J.; Klos, M. New Type of Device for Achievement of Grain Refinement in Metal Strip. Adv. Mater. Res. 2015, 1127, 91–97. [Google Scholar] [CrossRef]
  10. Rusz, S.; Klyszewski, A.; Salajka, M.; Hilser, O.; Cizek, L.; Klos, M. Possibilities of Application Methods Drece in Forming of Non-Ferrous Metals. Arch. Metall. Mater. 2015, 60, 3011–3015. [Google Scholar] [CrossRef] [Green Version]
  11. Totten, G.E.; Mackenzie, D.S. Handbook of Aluminum: Physical Metallurgy and Processes 1; CRC Press: Boca Raton, FL, USA, 2003; Volume 1. [Google Scholar]
  12. Mckenzie, P.W.J.; Lapovok, R. ECAP with back pressure for optimum strength and ductility in aluminium alloy 6016. Part 1: Microstructure. Acta Mater. 2010, 58, 3198–3211. [Google Scholar] [CrossRef]
  13. Tański, T.; Snopiński, P.; Pakieła, W.; Borek, W.; Prusik, K.; Rusz, S. Structure and properties of AlMg alloy after combination of ECAP and post-ECAP ageing. Arch. Civ. Mech. Eng. 2016, 16, 325–334. [Google Scholar] [CrossRef]
  14. Pandey, V.; Singh, J.K.; Chattopadhyay, K.; Santhi Srinivas, N.C.; Singh, V. Influence of ultrasonic shot peening on corrosion behavior of 7075 aluminum alloy. J. Alloys Compd. 2017, 723, 826–840. [Google Scholar] [CrossRef]
  15. Williamson, G.K.; Hall, W.H. X-ray line broadening from filed aluminium and wolfram. Acta Mater. 1953, 1, 22–31. [Google Scholar] [CrossRef]
  16. Cabibbo, M.; Paoletti, C.; Ghat, M.; Forcellese, A.; Simoncini, M. Post-FSW Cold-Rolling Simulation of ECAP Shear Deformation and Its Microstructure Role Combined to Annealing in a FSWed AA5754 Plate Joint. Materials 2019, 12, 1526. [Google Scholar] [CrossRef] [PubMed] [Green Version]
  17. Ungar, T.; Mughrabi, H.; Rönnpagel, D.; Wilkens, M. X-ray line-broadening study of the dislocation cell structure in deformed [001]-orientated copper single crystals. Acta Mater. 1984, 32, 333–342. [Google Scholar] [CrossRef]
  18. Howeyze, M.; Arabi, H.; Eivani, A.R.; Jafarian, H.R. Strengthening of AA5052 aluminum alloy by equal channel angular pressing followed by softening at room temperature. Mater. Sci. Eng. A 2018, 720, 160–168. [Google Scholar] [CrossRef]
  19. Dinkerl, M.; Pyczak, F.; May, J.; Hoppel, H.W.; Goken, M. Xrd profile analysis characterization of ultrafine grained Al-Mg alloys. J. Mater. Sci. 2009, 43, 7481–7487. [Google Scholar] [CrossRef]
  20. Liu, M.; Roven, H.J.; Liu, X.; Murashkin, M.; Valiev, R.Z.; Ungar, T.; Balogh, L. Grain refinement in nanostructured Al–Mg alloys subjected to high pressure torsion. J. Mater. Sci. 2010, 45, 4659–4664. [Google Scholar] [CrossRef]
  21. Zhang, C.; Wang, C.; Guo, R.; Zhao, G.; Chen, L.; Sun, W.; Wang, X. Investigation of dynamic recrystallization and modeling of microstructure evolution of an Al-Mg-Si aluminum alloy during high-temperature deformation. J. Alloys Compd. 2019, 773, 59–70. [Google Scholar] [CrossRef]
  22. Tański, T.; Snopiński, P.; Prusik, K.; Sroka, M. The effects of room temperature ECAP and subsequent aging on the structure and properties of the Al-3%Mg aluminium alloy. Mater. Charact. 2017, 133, 185–195. [Google Scholar] [CrossRef]
  23. Izairi, N.; Ajredini, F.; Vevecka-Priftaj, A.; Ristova, M. Enhancement of mechanical properties of the AA5754 aluminium alloy with a severe plastic deformation. Mater. Technol. 2014, 48, 385–388. [Google Scholar]
  24. León, J.; Salcedo, D.; Murillo, Ó.; Luis, C.J.; Fuertes, J.P.; Puertas, I.; Luri, R. Mechanical Properties Analysis of an Al-Mg Alloy Connecting Rod with Submicrometric Structure. Metals 2015, 5, 1397–1413. [Google Scholar] [CrossRef] [Green Version]
  25. Tang, L.; Peng, X.; Huang, J.; Ma, A.; Deng, Y.; Xu, G. Microstructure and mechanical properties of severely deformed Al-Mg-Sc-Zr alloy and their evolution during annealing. Mater. Sci. Eng. A 2019, 754, 295–308. [Google Scholar] [CrossRef]
  26. Khelfa, T.; Rekik, M.A.; Munoz-Bolanos, J.A.; Cabrera-Marrero, J.M.; Khitouni, M. Microstructure and strengthening mechanisms in an Al-Mg-Si alloy processed by equal channel angular pressing (ECAP). Int. J. Adv. Manuf. Technol. 2018, 95, 1165–1177. [Google Scholar] [CrossRef]
Figure 1. Principle of the dual rolls equal channel extrusion (DRECE) process.
Figure 1. Principle of the dual rolls equal channel extrusion (DRECE) process.
Materials 13 00301 g001
Figure 2. Microstructure of the 5754 aluminum alloy in an initial state.
Figure 2. Microstructure of the 5754 aluminum alloy in an initial state.
Materials 13 00301 g002
Figure 3. X-Ray diffraction profiles of 5754 aluminum alloy in different conditions.
Figure 3. X-Ray diffraction profiles of 5754 aluminum alloy in different conditions.
Materials 13 00301 g003
Figure 4. Examples of grain structures of 5754 aluminum alloy subjected to (a) one DRECE pass, (b) two DRECE passes, (c) three DRECE passes, (d) four DRECE passes, (e) five DRECE passes, (f) six DRECE passes.
Figure 4. Examples of grain structures of 5754 aluminum alloy subjected to (a) one DRECE pass, (b) two DRECE passes, (c) three DRECE passes, (d) four DRECE passes, (e) five DRECE passes, (f) six DRECE passes.
Materials 13 00301 g004
Figure 5. Electron backscattered diffraction (EBSD) inverse pole figure (IPF) maps of 5754 aluminum alloy (a) initial state, (b) one DRECE pass, (c) four DRECE passes, (d) six DRECE passes.
Figure 5. Electron backscattered diffraction (EBSD) inverse pole figure (IPF) maps of 5754 aluminum alloy (a) initial state, (b) one DRECE pass, (c) four DRECE passes, (d) six DRECE passes.
Materials 13 00301 g005
Figure 6. Misorientation distribution of the 5754 alloy samples (a) initial state, (b) one DRECE pass, (c) four DRECE passes, (d) six DRECE passes.
Figure 6. Misorientation distribution of the 5754 alloy samples (a) initial state, (b) one DRECE pass, (c) four DRECE passes, (d) six DRECE passes.
Materials 13 00301 g006
Figure 7. Hardness distribution along the sheet thickness of the 5754 aluminum alloy samples.
Figure 7. Hardness distribution along the sheet thickness of the 5754 aluminum alloy samples.
Materials 13 00301 g007
Figure 8. Examples of grain structures of 5754 aluminum alloy subjected to annealing for 30 min (a) 150 °C, (b) 180 °C, (c) 200 °C, (d) 250 °C, (e) 300 °C, and (f) 350 °C.
Figure 8. Examples of grain structures of 5754 aluminum alloy subjected to annealing for 30 min (a) 150 °C, (b) 180 °C, (c) 200 °C, (d) 250 °C, (e) 300 °C, and (f) 350 °C.
Materials 13 00301 g008
Figure 9. X-Ray diffraction profiles of DRECE processed and annealed 5754 aluminum alloy.
Figure 9. X-Ray diffraction profiles of DRECE processed and annealed 5754 aluminum alloy.
Materials 13 00301 g009
Table 1. Chemical composition of the 5754 aluminum alloy.
Table 1. Chemical composition of the 5754 aluminum alloy.
AlMgSiMnFeCrCuZnTi
Bal.2.6–3.6≤0.4≤0.5≤0.4≤0.3≤0.1≤0.2≤0.15
Table 2. Structural parameters of the 5754 aluminum alloy determined by X-ray diffraction peak analysis. Dv = domain size; ρd = dislocation density due to lattice microstrain; ρs = dislocation density due to size effect; ρ = total dislocation density.
Table 2. Structural parameters of the 5754 aluminum alloy determined by X-ray diffraction peak analysis. Dv = domain size; ρd = dislocation density due to lattice microstrain; ρs = dislocation density due to size effect; ρ = total dislocation density.
SampleDv(nm)ρ (m−2)ρd (m−2)ρ (m−2)
Initial state352.46∙× 10154.86∙× 10133.46 × 1014
322.98∙× 10151.40∙× 10146.47 × 1014
342.63∙× 10151.35 × 10145.96 × 1014
313.13 × 10151.04∙× 10145.73 × 1014
303.15 × 10151.67∙× 10147.25 × 1014
322.84 × 10151.50∙× 10146.54 × 1014
293.36 × 10151.69∙× 10147.55 × 1014
Table 3. Summarized results of the EBSD analysis.
Table 3. Summarized results of the EBSD analysis.
Grain Size (Intercept Lengths) [μm]Fraction of Low Angle Grain Boundaries, %Fraction of High Angle Grain Boundaries, %Average Misorientation Angle, θAV [°]
Initial state7.91611.688.436.98
7.86213.486.637.76
6.87241.458.625.50
6.95840.459.627.27
Table 4. Summary of mechanical properties of 5754 alloy.
Table 4. Summary of mechanical properties of 5754 alloy.
ConditionAverage Vickers MicrohardnessYield Strength (MPa)Tensile Strength (MPa)Elongation, %
Initial state79.6112.321630.1
91.7184.7235.413.2
93.6188.1239.510.6
93.7189.4241.210.0
96.3193.3246.19.1
97.5194.1247.09.0
99.5198.2251.88.4
Table 5. Structural parameters of the DRECE processed and annealed 5754 aluminum alloy determined by X-ray diffraction peak analysis. Dv = domain size; ρd = dislocation density due to lattice microstrain; ρs = dislocation density due to size effect; ρ = total dislocation density.
Table 5. Structural parameters of the DRECE processed and annealed 5754 aluminum alloy determined by X-ray diffraction peak analysis. Dv = domain size; ρd = dislocation density due to lattice microstrain; ρs = dislocation density due to size effect; ρ = total dislocation density.
Annealing Temperature [°C]Dv (nm)ρs (m−2)ρd (m−2)ρ (m−2)
150342.50 × 10158.75 × 10134.68 × 1014
180362.31 × 10158.51 × 10134.44 × 1014
200372.14 × 10158.06 × 10134.16 × 1014
250431.61 × 10158.63 × 10133.73 × 1014
300401.85 × 10152.27 × 10132.05 × 1014
350471.35 × 10157.48 × 10133.18 × 1014
Table 6. Average hardness values of DRECE processed and annealed 5754 alloy.
Table 6. Average hardness values of DRECE processed and annealed 5754 alloy.
Annealing Temperature [°C]Average Vickers Microhardness
15081.5
18074.1
20077.1
25061.1
30061.5
35068.7

Share and Cite

MDPI and ACS Style

Snopiński, P.; Tański, T.; Gołombek, K.; Rusz, S.; Hilser, O.; Donič, T.; Nuckowski, P.M.; Benedyk, M. Strengthening of AA5754 Aluminum Alloy by DRECE Process Followed by Annealing Response Investigation. Materials 2020, 13, 301. https://doi.org/10.3390/ma13020301

AMA Style

Snopiński P, Tański T, Gołombek K, Rusz S, Hilser O, Donič T, Nuckowski PM, Benedyk M. Strengthening of AA5754 Aluminum Alloy by DRECE Process Followed by Annealing Response Investigation. Materials. 2020; 13(2):301. https://doi.org/10.3390/ma13020301

Chicago/Turabian Style

Snopiński, Przemysław, Tomasz Tański, Klaudiusz Gołombek, Stanislav Rusz, Ondřej Hilser, Tibor Donič, Paweł M. Nuckowski, and Marcin Benedyk. 2020. "Strengthening of AA5754 Aluminum Alloy by DRECE Process Followed by Annealing Response Investigation" Materials 13, no. 2: 301. https://doi.org/10.3390/ma13020301

APA Style

Snopiński, P., Tański, T., Gołombek, K., Rusz, S., Hilser, O., Donič, T., Nuckowski, P. M., & Benedyk, M. (2020). Strengthening of AA5754 Aluminum Alloy by DRECE Process Followed by Annealing Response Investigation. Materials, 13(2), 301. https://doi.org/10.3390/ma13020301

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop