Article

Evaluating Cement Treated Aggregate Base Containing Steel Slag: Mechanical Properties, Volume Stability and Environmental Impacts

1
Engineering Research Center of Catastrophic Prophylaxis and Treatment of Road & Traffic Safety of Ministry of Education, Changsha University of Science & Technology, Changsha 410114, China
2
School of Traffic and Transportation Engineering, Changsha University of Science and Technology, Changsha 410114, China
3
Power China Guiyang Engineering Co., Ltd., Guiyang 550000, China
*
Author to whom correspondence should be addressed.
Materials 2022, 15(23), 8277; https://doi.org/10.3390/ma15238277
Submission received: 25 August 2022 / Revised: 10 October 2022 / Accepted: 8 November 2022 / Published: 22 November 2022
(This article belongs to the Section Construction and Building Materials)

Abstract

:
Steel slag has been commonly used in road engineering as cementitious material; however, its application in base course is not widely reported. Four contents of steel slag (0%, 30%, 50%, 75% by volume) were blended into different cement (3%, 4%, 5%, 6% by weight)-treated aggregates. Mechanical properties, volume stability, economic benefits and environmental influences of steel slag mixtures were investigated for the feasibility of applying steel slag in semi-rigid base course. Abrasion, crushing and elongated particle content were compared against limestone aggregate, showing that steel slag has the potential of replacing natural aggregate in concrete. Steel slag is beneficial for reinforcement of the strength and stiffness. The mixture has the highest strength and stiffness when bended with 50% steel slag at 4% cement content. By treating steel slag with CH3COOH or adding silica fume, volume expansion of steel slag can effectively be controlled. Larger size steel slag (>4.75 mm) and higher cement content are recommended due to heavy metal leaching risk, especially in salty humid areas. Steel slag has sound economic benefits due to the relatively low price. Environmental benefits can also be achieved given that the transport CO2eq emission of steel slag is accounted for. With proper control in production process, steel slag is a very promising alternative material to be utilized in cement-stabilized base course in road engineering.

1. Introduction

Road infrastructure in China has experienced a fast development in the past three decades. The total mileage of motorway is over 5 million kilometers at the end of 2021, including nearly 160 thousand kilometers of high-speed expressway [1]. In the meantime, about 800 thousand kilometers of motorway needs rehabilitation or maintenance each year. A large number of aggregates are required to meet the needs of new constructions and maintenances, rendering a huge burden on natural resource and environment protection. There are urgent needs for sustainable and environmental substitute for natural aggregates in road engineering. At the same time, industrial wastes have increased as a result of rising population and technological development, posing increasingly serious social problems and environmental threats. Innovative approaches have been studied to decrease these wastes, or, as a clearer option, turn them into valuable reserves [2,3]. For several decades, various industry wastes have been extensively studied to replace aggregates or to enhance performance of construction materials [4,5,6].
Steel slag is one of the by-products generated in steel making process. China’s crude steel production reaches 1.03 billion tons in 2021 [1]. According to production rate of 60~150 kgt−1 based on the current refining processes, the steel slag production is around 60~150 million tons yearly. A huge quantity of steel slag needs to be handled properly. Nevertheless, compared to 85~98% of utilization rate in industrialized countries such as USA, Europe and Japan, the utilization in China is only at 29.5% [7]. Most of it is piled up or disposed as landfill, which not only occupies land resource, but also causes leaking of harmful component.
The physic properties of steel slag, i.e., hardness, crushing and grinding, makes it adequate for road engineering. If used appropriately, steel slag can partially or fully replace aggregates in mixtures; not only can the shortage of construction resources be alleviated, but also the damage to environment can be reduced. The utilization of steel slag for road construction in the United States is at nearly 50%; in Europe at 43%, and in Japan at 32.4%, whilst in China it is only at 7.6% [7]. Much work has been done to apply steel slag in asphalt pavement in recent years. He et al. and Skaf et al. have argued that road construction is the most effective and lowest-cost way to utilize steel slag [8,9]. Studies have suggested that electric steel slag displayed almost the same mechanical and physical properties as traditional aggregates [10,11]. Scholars have also found that steel slag can improve high temperature performance [12,13], moisture stability [14] and fatigue [15] of asphalt mixture significantly. Moreover, the solutions to obtain functional pavement such as improving skid resistance [16], deicing [17] and self-healing material [18] became more vital and diverse with the application of steel slag. In addition, the utilization of steel slag mixtures has sound economic benefit and potential environmental benefits compared to traditional mineral aggregate mixtures [19,20,21]. Despite the many merits of steel slag over natural aggregates, the applications of steel slag in paving material are still conservative. Concerns include physical and morphologic property, replacement content, long-term volume stability and environmental impacts [22,23,24].
Previous studies on steel slag in road engineering mainly focus on asphalt mixture and surface course, relatively few on applications of incorporating steel slag in base layer. Based on the reality that cement-stabilized base is the main base type, and the massive slag waste in China at this stage and beyond, the utilizing of steel slag in cement-stabilized base was investigated in this study. We designed four levels of replacement: 0%, 30%, 50% and 75% of steel slag, and the optimal moisture contents were determined through compaction test. Performances of samples with different steel slag contents were evaluated. Unconfined compressive strength, bending strength and resilient modulus were tested for mechanical properties. Volume expansion of steel slag and dry shrinkage of steel slag mixture were also checked. Environmental impacts were evaluated in view of heavy metal leaching and carbon footprint. Other means including SEM, X-ray and FAAS were also employed to check the surface morphology, element distribution and chemical composition to comprehend the strength development and environmental impacts of steel slag in cement-stabilized semi-rigid base.

2. Materials and Specimen

2.1. Materials

The steel slag used in this study was obtained from Shenglong Steel Mill and the limestone was from a quarry, in Fangchenggang, Guangxi, China, as displayed in Figure 1. Cement of 42.5 MPa was produced by Runfeng. Physical and mechanical properties of steel slag and limestone are compared in Table 1. As properties of steel slag would change with aging time, samples were examined at different aging times, namely, 0 months, 6 months and 12 months. Although decreasing slightly with aging time and varying with particle size, the apparent density of steel slag is about 25~36% higher than that of limestone. At the same time, crushing, abrasion and elongated particle content of steel slag are smaller than those of limestone. Water absorption of steel slag is higher, which can be explained by the porous surface shown in the multi-scale images by Scanning Electron Microscopy (SEM) in Figure 2. However, the water absorption decreases with aging time. Table 2 records the chemical compositions of steel slag through an X-ray fluorescence semi-quantitative analysis. The most prominent component is CaO, followed by Fe2O3 and SiO2, accounting for about 84% altogether. It is notable that f-CaO and f-MgO experience steady declines with aging time. Metal constitutes of the steel slag were detected with grinded steel slag powder (<0.125 μm) by the Flame Atomic Absorption Spectrophotometer (FAAS). Heavy metal elements of steel slag with 12 months of aging are displayed in Figure 3. Mn, Cr and V are the top 3 heavy metals.

2.2. Mixture Design and Specimen Preparation

The particle sizes of steel slag on site mainly lie between 4.75 mm~19 mm, as Figure 1 shows. Due to the differences of density between steel slag and limestone, volume was chosen as an indicator for steel slag replacement. Thus, a volume–mass conversion was performed on aggregates of steel slag and limestone. The composite gradation of “steel slag + limestone” mixture in 0.45 power chart is illustrated in Figure 4.
Cement-treated aggregates with four steel slag contents of 0% (control group), 30%, 50%, 75% and four cement contents of 3%, 4%, 5%, 6% were formulated. The samples of different steel slag contents were compacted using impaction test method as per JTG E51-2009 [25] to determine the relationship between water content and dry density. The determined optimum moisture content (OMC) and maximum dry density (MDD) are listed in Table 3. With steel slag content growing, the OMCs and MDDs of mixture increase. OMC of samples with 50% steel slag is about 30% higher than that of the control group.
The cylindrical specimens with dimension of Φ 150 mm × 150 mm were adopted for unconfined compressive strength (UCS), unconfined compressive resilient modulus (UCRM) and volume expansion tests. Prism specimens with dimension of 100 mm × 100 mm × 400 mm were used for bending strength (BS) and dry shrinkage tests. The samples were controlled at 98% compactness and at least four duplicates were prepared for each test. Samples for UCS and dry shrinkage test were cured in standard condition (temperature of 20 ± 1 °C, humidity of 95 ± 5%) for 7 days, while samples for UCRM and BS test were cured for 28 days. The production and curing process of samples are shown in Figure 5.

3. Methodology

3.1. Mechanical Test

To investigate the influence of steel slag on strength and stiffness, the UTM-100 servo-hydraulic multi-functional material test system was employed to test unconfined compressive strength (UCS), bending strength (BS) and unconfined compressive resilient modulus (UCRM). When the samples were subjected to UCS test, the loading rate was set to 1 mm/min, while in the BS test, the loading rate was set to 50 mm/min, as per JTG E51-2009 [25]. For the UCRM test, the specimens were subjected to five loading levels, with the maximum load of 65% of the strength, as per JTG E51-2009 [25]. The mechanical tests are shown in Figure 6.

3.2. Volume Stability Test

The volume stability test consists of two parts: the volume expansion of steel slag and the dry shrinkage of cement-stabilized aggregates containing steel slag. The safety of highway is affected by the possible expansion caused by f-CaO and f-MgO in steel slag. Steel slag with no aging was compacted at OMC, and soaked in water in the mold with permeable platters at each end. Dial directors were set to monitor the volume increase for 10 consecutive days. Samples treated with CH3COOH or silica fume were also tested to clarify their inhibition effect on volume expansion. To explore the shrinkage of mixture with different steel slag contents, after curing in standard condition for 7 days, prism samples were examined for initial mass and length and then set in a condition of 20 ± 1 °C and 60 ± 5 % humidity with both ends measured with dial directors to monitor the length change due to dry shrinkage. The mass and length of samples were recorded every day during the first 7 days, every other day from 7th to 28th day, and on the 60th and 90th day. In the end, the specimens were heated to constant weight. Length and mass of the final state were measured. The volume expansion of steel slag and dry shrinkage of cement concrete with steel slag are in Figure 7.

3.3. Heavy Metal Leaching Test

The heavy metal pollution of steel slag was examined through precipitation of Cr and V. Influence of particle size, cement content and water salinity were evaluated. An amount of 100 g of steel slag with different particle size from less than 0.075 mm to larger than 26.5 mm (Figure 8a) was put into 200 mL pure water for 24 h. To check the influence of cement content on metal precipitation, samples of Φ 150 mm ×150 mm containing 50% steel slag with 4%, 5% and 6% cement content (Figure 8b) were prepared and put into 3250 mL pure water to be fully emerged. A control group with no steel slag was examined as well. As Fangchenggang is a coastal city in southern China, heavy metal precipitation in seawater environment was also checked. To eliminate size effect, the steel slag aggregates were grinded into powder, and 100 g samples were put in 200 mL water of 0%, 0.5%, 1%, 1.5%, 2%, 2.5% salinity (Figure 8c). Change of heavy metal in the water was detected every 4 h for a total duration of 24 h.

3.4. Economic Evaluation and Carbon Footprint Simulation

A case study of cement-stabilized aggregate base course for a typical four-lane highway with a dimension of 1 km long, 20 cm thick and 32 m wide was conducted to investigate economic gains and greenhouse gas (GHG) emissions. In the definition of cement-treated aggregates, mainly Portland cement and gravel constitute the composition. Water is not considered in the subsequent calculation due to its small amount. The consumptions of steel slag, limestone aggregate and cement were determined based on the compaction experiments (Table 3). Market prices of raw materials were surveyed. In the transportation cost calculation, compared to the commonly seen natural aggregate quarries located in many parts of the country, steel slag appears only in fixed steel mills. Silica fume is also hauled long distance from manufactories. As a result, the average transport distance of 40 km for cement, 40 km for limestone, 100 km for steel slag and silica fume were assumed.
To further compare the environmental impacts of cement-stabilized aggregate with steel slag in the aspect of equivalent CO2 (CO2eq) emission, life cycle analysis (LCA) models of cement-stabilized aggregate base course were prepared with SimaPro 9 software. The methodology of LCA consists of 4 stages including goal and scope of the project, inventory analysis, impact assessment and interpretation of results. Correspondently, the research methodology followed for this research is represented in Figure 9. Consumption of natural resources and CO2eq emission for mix preparation is considered the project’s goal and scope. In inventory analysis, binder materials and aggregates are considered from the Ecoinvent database as per European standards. In the LCA assembly stage, for mix preparation, all the binders, minerals and steel slags are evaluated as per the mix compaction as indicated in Table 3. Since steel slag is recycled as a by-product of steelmaking, the energy consumption of producing steel slag is zero. The only major environmental impact of steel slag is the transport process. Table 4 collects the energy consumption data for cement and limestone production life cycle analysis (LCA) [19]. In the impact assessment, the ReCiPe 2016 midpoint method was used in SimaPro for LCA [26,27,28]. The mid-point implications include climate change challenges, human toxicity, loss of the ozone layer, acidification, and abiotic capital depletion, and is classified as more precise. Electricity was the final contribution to the mix phase. Energy is necessary to blending the ingredients to obtain the end product. The shipping of the material was also taken into account, by 32-ton trucks. The average transport distance of 40 km for cement, 40 km for limestone, 100 km for steel slag and silica fume were assumed. Global and European database values available in SimaPro 8.4 were used to characterize and normalize the environmental impacts of the products.

4. Results and Discussions

4.1. Mechanical Properties

The UCS (Figure 10a), BS (Figure 10b) and UCRM (Figure 10c) are overall positively related to cement content and steel slag: with steel slag replacement content increasing, UCS and BS keep climbing until reaching its peak at 50% replacement, followed by a small decrease. The average UCS of 4% cement treated aggregates without steel slag is 3.73 MPa, comparatively, UCS of specimens with 30% steel slag is 4.33 MPa, about 15% higher, met the strength requirement of cement-stabilized base for heavy traffic pavement (4.0~6.0 MPa) [29]. Especially when steel slag content is at 50%, the UCS is around 5.4 MPa, meeting the strength requirement of cement-stabilized base for extremely heavy traffic pavement (5.0~7.0 MPa) [29]. In other words, steel slag could be applicated in cement-stabilized base for heavy traffic pavement.
In general, when steel slag content increases from 0 to 50%, the strength and stiffness increases. This is because steel slag is a very strong material with rough surface that strengthens the particle extrusion, which helps form a strong aggregate skeleton to increase the resistance to damage. Moreover, the cementitious components of C3S/C2S contained in steel slag are hydrated to obtain C-S-H gel [30], which constitutes the fundamental building block of hydrated cement and makes the system stronger:
2(3CaO·SiO2) + 6H2O→3CaO·2SiO2·3H2O + 3Ca(OH)2,
2(2CaO·SiO2) + 4H2O→3CaO·2SiO2·3H2O + Ca(OH)2.
In the event that gypsum is present in cement clinker, C3A would also react with CaSO4 to form trisulfide calcium aluminate hydrate (C6AS3H32). The internal voids of cement slurry and surface porosity of steel slag are filled with these two hydration products, and the bonding effect of cement particle is improved. Apparently, the cementitious components contained in steel slag would help increase the hydration products, thereby reinforcing the mechanical performance and durability of the mixture.
However, when the content of steel slag further increases, the high porosity of steel slag increases the voids in the sample. Some of the cement would be adsorbed and wrapped in the surface porosity of steel slag and insulate from further hydration reaction, which is unbeneficial to the strength formation. In this study, when steel slag increases from 50% to 75%, the 7d UCS experienced a decline of 6~14%, and 28 UCRM a decline of 14~18%, indicating that the adverse effects of porosity began to overtake the positive effects of rough surface and gelling composition when replacement content of steel slag is too high. The recommended steel slag replacement is about 50% based on the test results in this study.

4.2. Volume Stability

4.2.1. Volume Expansion of Steel Slag

The volume changes of steel slag are displayed in Figure 11. As is shown, the volume of steel slag increases sharply with immerging time. This is mainly due to the reaction of f-CaO contained in steel slag with water. The volume expansion can be significantly reduced by treating the steel slag with CH3COOH or adding silica fume. As can be seen, the volume expansion has a negative relation with CH3COOH concentration or silica fume content. In this study, volume expansion of steel slag treated with 15% CH3COOH or 4.8% silica fume is reduced very close to 0%. However, the expansion rises again when silica fume is increased to 9.6%; the excessive silica fume downgrades the skeleton structure of aggregate and decreases the interlock of aggregates. To assure the volume stability in the long run, it is recommended that the content of silica fume should be strictly controlled, preferably around 4.5%.
To ensure long-term performance, there are several recommendations to control the possible expansion of steel slag: Firstly, steel slag should be detected for active substances (free calcium oxide or free magnesium oxide). Unreliable source of steel slag with high content of f-CaO or f-MgO should not be used. Secondly, steel slag needs to be treated to mitigate the expansion effects, either by aging for a period of time (as indicated that f-CaO or f-MgO of steel slag steadily decline with aging time in Table 2), or treated with appropriate CH3COOH or silica fume. Moreover, adding silica fume to steel slag during production process when it is still in liquid molten state is an effective solution [21].

4.2.2. Shrinkage of Steel Slag Mixture

The recorded weight and length change of cement-stabilized mixes were employed to calculate the moisture loss and shrinkage coefficients (Equations (3) and (4)).
ω i = m i m i + 1 m c
α d = ε i ω i
where εi is the shrinkage strain; ωi is the moisture loss rate; mi is the specimen weight; mc is the constant dry weight of specimen; αd is the shrinkage coefficient.
Cumulative moisture loss rates and shrinkage coefficients and represented in Figure 12. The moisture loss increases fast for the first few days because of free water evaporation. The moisture loss at stable stage (after 30 days) of samples with 50% steel slag is much higher than those with no steel slag, reflecting the fact that higher steel slag content corresponds to higher water loss due to the higher water content. This reminds us that more attention should be given to the moisture maintenance of cement-stabilized base with steel slag in the first 1~2 weeks to reduce moisture loss. Then, it began to climb slowly. This stage is the gradual bound water loss with time. After about 30 days, the water loss becomes stable. It is found that steel slag inhibits the drying shrinkage: the shrinkage coefficients decrease at higher steel slag content. The final shrinkage coefficients of samples with 50% of steel slag are about 40% less than the control group. It is also evident in previous research that the expansion caused by f-CaO and f-MgO contained in steel slag may counteract partial shrinkage [31].

4.3. Heavy Metal Leaching

Cr and V leaching of different particle sizes are listed in Table 5 and Table 6. It is clearly shown that heavy metal leaching of small particle size is much higher than that of large ones. Cr precipitations of 4.75~9.5 mm, 9.5~19 mm, 19~26.5 mm particles are 60%, 67% and 71% lower than of those passing 0.075 mm, respectively. V precipitations of 4.75~9.5 mm, 9.5~19 mm, 19~26.5 mm particles are about 40%, 60% and 64% lower than of those passing 0.075 mm, respectively. Small particle size has higher specific surface area, meaning more contact area with water. In this sense, it is recommended that steel slag used in cement-stabilized base be not smaller than 4.75 mm.
Precipitations of Cr and V with different cement content are shown in Figure 13. The precipitation of heavy metal decreased significantly after being mixed with cement, as more cement mortar provides better coverage and inhibits heavy metal from leaching into surrounding environment. Compared to 4% cement, precipitation of Cr and V at 6% cement declined about 25% and 35%, respectively.
The precipitation of heavy metal was also checked in salty water. The salinity of sea water nearby Fangchenggang is about 2%. Figure 14 demonstrates that 24 h cumulative precipitation of Cr and V at 2% salt water are nearly threefold and double those in pure water, respectively. The active ions contained in salty water can react with the metal ions in steel slag, and also would corrode the covering cementitious material which in turn promotes heavy metal precipitation. When utilized in salty water environment, stricter measurements should be implemented to prevent possible heavy metal pollution.

4.4. Economic and Carbon Footprint Analysis

Steel slag has shown sound performance following similar procedures of pavement engineering; the economic cost and greenhouse gas (GHG) emission are two other aspects to check. The material and transport costs were calculated for 50% and 30% steel slag replacement, as shown in Table 7. Due to the low price of steel slag, the total costs of steel slag mixture can be saved approximately by about 22% (50% steel slag replacement) and 15% (30% steel slag replacement). Even with 3% silica fume added, the total costs can still be economized by 12% and 10%, respectively, indicating that the steel slag has sound economic gains.
The CO2eq emission of different steel slag contents were displayed in Figure 15, Figure 16, Figure 17 and Figure 18. As shown in Figure 15, Figure 16 and Figure 17, for 1 P of cement-stabilized limestone aggregate base course (1 km long by 20 cm thick by 32 m wide), the CO2eq emission is 3.06 × 105 kg. Comparatively, the CO2eq emissions of 1 P of “30% steel slag +70% limestone” and “50% steel slag + 50% limestone” base course are 3.18 × 105 kg and 3.37 × 105 kg, respectively. It is found that in the initial assumption of 100 km transport distance for steel slag the total CO2eq emissions of “steel slag + limestone” mixtures actually are higher than the traditional limestone concrete. The corresponding CO2eq emissions for each procedure in the mixture production are summarized in Figure 18. Cement production contributes the most CO2eq emission, accounting for nearly 60% of the total emission. This adheres to our ordinary expectation that energy consumption and pollution from cement production is very high. Unlike the overall life cycle, economic performance is usually less sensitive to transport distance [32], CO2eq emission from material transport is non-neglectable, and it grows with steel slag replacement. For instance, the CO2eq emission from material (mainly steel slag) transport accounts for as high as 30% of the total emission for the “50% steel slag + 50% limestone” mixture. The environmental impacts of steel slag depend on the weight of steel slag as well as its haul distance. In this sense, we further calculated the critical transport distance. The critical transport distance is 59 km for “50% steel slag + 50% limestone” mixture, and 74 km for “30% steel slag +70% limestone” mixture. That is, environmental benefits can be achieved if the transport distance is below 59 km for “50% steel slag + 50% limestone” mixture, and below 74 km for “30% steel slag + 70% limestone” mixture.

5. Conclusions

Steel slag is a promising alternative for natural aggregates in pavement base course. In this study, different steel slag content (0%, 30%, 50%, 75%) was added to cement-treated aggregates. Throughout investigations including mechanical properties, volume characterization, economic benefits and environmental impacts, main conclusions are as follows:
(1)
Compared to traditional mineral aggregate (i.e., limestone), steel slag aggregate has equal or superior engineering properties, including density, abrasion resistance and crushing resistance. Due to higher water absorption and larger gravity, the OMC and MDD increase proportionally as more natural aggregates are replaced with steel slag.
(2)
Mechanical properties including strength and stiffness are significantly improved by steel slag within 50% replacement due to the increased hydration products and interlocked aggregate structure. However, the porosity and water absorption rate have greater negative effect on strength when steel slag replacement further increases.
(3)
Appropriate treatment with CH3COOH or addition of silica fume can relieve the volume expansion of steel slag. Nevertheless, excessive silica fume may be detrimental to the aggregate structure and should be kept within a reasonable content: 3–4.5%.
(4)
Smaller particle size shows higher risk of heavy metal precipitation, and the salty water environment in coastal area adds to it. Large particle size (>4.75 mm) and higher cement content are recommended to reduce heavy metal leaching threat.
(5)
Steel slag mixture has sound economic gains and potential environmental benefits compared to limestone mixture. However, the transport emission of steel slag should be accounted for to determine an environmental haul distance of steel slag.
Further research would be focused on long-term performances of cement-treated aggregate base containing steel slag in real pavement projects in both the theoretic and engineering aspects.

Author Contributions

Y.H.: Investigation, Formal analysis, Methodology, Writing-original draft, Funding acquisition; X.Y.: Investigation, Data curation, Formal analysis; S.W.: Investigation, Data curation; Z.L.: Conceptualization, Supervision, Resources, Funding acquisition. L.L.: Conceptualization, Project administration, Writing-review and editing; B.X.: Laboratory test, Data curation. All authors have read and agreed to the published version of the manuscript.

Funding

This work was supported by National Natural Science Foundation of China (52008044); Natural Science Foundation of Hunan Province (2022JJ40479); Excellent Youth Project by Department of Education of Hunan Province (21B0296); Open Fund of Engineering Research Center of Catastrophic Prophylaxis and Treatment of Road & Traffic Safety of Ministry of Education (Changsha University of Science & Technology) (kfj210401).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Conflicts of Interest

The authors declare that they have no conflict of interest, and no competing financial interests or personal relationships that could have appeared to influence the work reported in this paper.

References

  1. National Bureau of Statistics of China. Crude Steel Output. 2021. Available online: http://data.stats.gov.cn (accessed on 25 August 2022).
  2. Mesci, B.; Çoruh, S.; Ergun, O.N. Use of Selected Industrial Waste Materials in Concrete Mixture. Environ. Prog. Sustain. Energy 2011, 30, 368–376. [Google Scholar]
  3. Ahmad, J.; Zhou, Z.; Martínez-García, R.; Vatin, N.I.; De-Prado-Gil, J.; El-Shorbagy, M.A. Waste Foundry Sand in Concrete Production Instead of Natural River Sand: A Review. Materials 2022, 15, 2365. [Google Scholar] [CrossRef] [PubMed]
  4. Ahmad, J.; Martínez-García, R.; De-Prado-Gil, J.; Irshad, K.; El-Shorbagy, M.A.; Fediuk, R.; Vatin, N.I. Concrete with Partial Substitution of Waste Glass and Recycled Concrete Aggregate. Materials 2022, 15, 430. [Google Scholar] [CrossRef] [PubMed]
  5. Kongar-Syuryun, C.; Tyulyaeva, Y.; Khairutdinov, A.M.; Kowalik, T. Industrial waste in concrete mixtures for construction of underground structures and minerals extraction. IOP Conf. Ser. Mater. Sci. Eng. 2020, 869, 032004. [Google Scholar] [CrossRef]
  6. Taskin, A.; Fediuk, R.; Grebenyuk, I.; Elkin, O.; Kholodov, A. Effective Cement Binders on Fly and Slag Waste from Heat Power Industry of the Primorsky Krai, Russian Federation. Int. J. Sci. Technol. Res. 2020, 9, 3509–3512. [Google Scholar]
  7. Guo, J.; Bao, Y.; Wang, M. Steel slag in China: Treatment, recycling, and management. Waste Manag. 2018, 78, 318–330. [Google Scholar] [CrossRef]
  8. He, L.; Zhan, C.; Lu, S.; Gao, J.; Xie, J.; Ling, T. Application status of steel slag asphalt mixture. J. Traffic Transp. Eng. 2020, 20, 15–33. [Google Scholar]
  9. Skaf, M.; Manso, J.; Aragon, A.; Fuente-Alonso, J.A.; Ortega-López, V. EAF slag in asphalt mixes: A brief review of its possible re-use. Resour. Conserv. Recycl. 2017, 120, 176–185. [Google Scholar] [CrossRef]
  10. Martins, A.; Carvalho, J.; Costa, J. Steel slags in cement-based composites: An ultimate review on characterization, applications and performance. Constr. Build. Mater. 2021, 291, 123265. [Google Scholar] [CrossRef]
  11. Passeto, M.; Baliello, A.; Giacomello, G.; Pasquini, E. Sustainable solutions for road pavements: A multi-scale characterization of warm mix asphalts containing steel slags. J. Clean. Prod. 2017, 166, 835–843. [Google Scholar] [CrossRef]
  12. Wen, H.; Wu, S.; Bhusal, S. Performance evaluation of asphalt mixes containing steel slag aggregates as a measure to resist studded tire wear. J. Mater. Civ. Eng. 2016, 28, 1–7. [Google Scholar] [CrossRef]
  13. Chen, J.; Wei, S. Engineering properties and performance of asphalt mixtures incorporating steel slag. Construct. Build. Mater. 2016, 128, 148–153. [Google Scholar] [CrossRef]
  14. Passeto, M.; Baliello, A.; Giacomello, G.; Pasquini, E. Rheological characterization of warm modified asphalt mastics containing electric arc furnace steel slag. Adv. Mater. Sci. Eng. 2016, 3, 1–11. [Google Scholar] [CrossRef] [Green Version]
  15. Shen, A.; Yu, M.; Guo, Y.; Cui, T.; Liu, B. Fatigue properties and improvement mechanism of steel slag asphalt mixture. J. Build. Mater. 2018, 21, 327–334. [Google Scholar]
  16. Cui, P.; Wu, S.; Xiao, Y.; Yang, C.; Wang, F. Enhancement mechanism of skid resistance in preventive maintenance of asphalt pavement by steel slag based on micro-surfacing. Constr. Build. Mater. 2020, 239, 117870. [Google Scholar] [CrossRef]
  17. Gao, J.; Sha, A.; Wang, Z.; Tong, Z.; Liu, Z. Utilization of steel slag as aggregates in asphalt mixtures for microwave deicing. J. Clean. Prod. 2017, 152, 429–442. [Google Scholar] [CrossRef]
  18. Sun, Y.; Wu, S.; Liu, Q.; Zeng, W.; Chen, Z.; Ye, Q.; Pan, P. Self-healing performance of asphalt mixtures through heating fibers or aggregates. Construct. Build. Mater. 2017, 150, 673–680. [Google Scholar] [CrossRef]
  19. Anastasiou, E.K.; Liapis, A.; Papayianni, I. Comparative life cycle assessment of concrete road pavements using industrial by-products as alternative materials. Resour. Conserv. Recycl. 2015, 101, 1–8. [Google Scholar] [CrossRef]
  20. Chen, X.; Wang, H.; Najm, H.; Venkiteela, G.; Hencken, J. Evaluating engineering properties and environmental impact of pervious concrete with fly ash and slag. J. Clean. Prod. 2019, 237, 117714. [Google Scholar] [CrossRef]
  21. Liu, J.; Yu, B.; Wang, Q. Application of steel slag in cement treated aggregate base coarse. J. Clean. Prod. 2020, 269, 121733. [Google Scholar] [CrossRef]
  22. Guimaraes, A.; Costa, K.; Reis, M.; Santana, C.S.A.; Castro, C.D. Study of controlled leaching process of steel slag in soxhlet extractor aiming employment in pavements. Transp. Geotech. 2021, 27, 100485. [Google Scholar] [CrossRef]
  23. Swathi, M.; Andiyappan, T.; Guduru, G.; Reddy, M.A.; Kuna, K.K. Design of asphalt mixes with steel slag aggregates using the Bailey method of gradation selection. Constr. Build. Mater. 2021, 279, 122426. [Google Scholar] [CrossRef]
  24. Xu, F.; Chen, Z.; Zhu, J.; Zhou, M.; Shen, W.; Chen, J. Research on the volume stability performance of steel slag road base materials. Concrete 2012, 9, 59–62. [Google Scholar]
  25. Department of Transportation. Test Methods Of Materials Stabilized With Inorganic Binders For Highway Engineering, JTG E51-2009; China Communications Press: Beijing, China, 2009.
  26. Manjunatha, M.; Preethi, S.; Malingaraya, H.G.; Mounika, H.; Niveditha, K. Life cycle assessment (LCA) of concrete prepared with sustainable cement-based materials. Mater. Today Proc. 2021, 47, 3637–3644. [Google Scholar] [CrossRef]
  27. O’Born, R. Life cycle assessment of large scale timber bridges: A case study from the world’s longest timber bridge design in Norway. Transp. Res. Part D Transp. Environ. 2019, 59, 301–312. [Google Scholar] [CrossRef]
  28. Goedkoop, M.; Oele, M.; Vieira, M.; Leijting, J.; Ponsioen, T.; Meijer, E. SimaPro Tutorial; Creative Commons: San Francisco, CA, USA, 2016. [Google Scholar]
  29. Department of Transportation. Specification For Design Of Highway Asphalt Pavement, Jtg D50-2017; China Communications Press: Beijing, China, 2017.
  30. Liu, L.; Zhou, A.; Deng, Y.; Cui, Y.; Yu, Z.; Yu, C. Strength performance of cement/slag-based stabilized soft clays. Construct. Build. Mater. 2019, 211, 909–918. [Google Scholar] [CrossRef]
  31. Wang, G.; Wang, Y.; Gao, Z. Use of steel slag as a granular material: Volume expansion prediction and usability criteria. J. Hazard. Mater. 2010, 184, 555–560. [Google Scholar] [CrossRef]
  32. Ferreira, V.J.; Saez-De-Guinoa Vilaplana, A.; García-Armingol, T.; Aranda-Usón, A.; Lausín-González, C.; López-Sabirón, A.M.; Ferreira, G. Evaluation of the steel slag incorporation as coarse aggregate for road construction: Technical requirements and environmental impact assessment. J. Clean. Prod. 2016, 130, 175–186. [Google Scholar] [CrossRef]
Figure 1. Aggregates of limestone and steel slag.
Figure 1. Aggregates of limestone and steel slag.
Materials 15 08277 g001
Figure 2. Multi-scale structure of steel slag by SEM.
Figure 2. Multi-scale structure of steel slag by SEM.
Materials 15 08277 g002
Figure 3. Heavy metal components of steel slag.
Figure 3. Heavy metal components of steel slag.
Materials 15 08277 g003
Figure 4. Mixture gradation.
Figure 4. Mixture gradation.
Materials 15 08277 g004
Figure 5. Specimen preparation and curing.
Figure 5. Specimen preparation and curing.
Materials 15 08277 g005
Figure 6. Mechanical properties test.
Figure 6. Mechanical properties test.
Materials 15 08277 g006
Figure 7. Volumetric properties test.
Figure 7. Volumetric properties test.
Materials 15 08277 g007
Figure 8. Heavy metal leaching test. (a) Steel slag aggregates of different particle size; (b) Samples with different cement content; (c) Containers with different seawater salinity.
Figure 8. Heavy metal leaching test. (a) Steel slag aggregates of different particle size; (b) Samples with different cement content; (c) Containers with different seawater salinity.
Materials 15 08277 g008aMaterials 15 08277 g008b
Figure 9. Virtual process for the cement-stabilized aggregate mix preparation.
Figure 9. Virtual process for the cement-stabilized aggregate mix preparation.
Materials 15 08277 g009
Figure 10. Mechanical properties of mixtures with steel slag. (a) UCS at 7 d; (b) BS at 28 d; (c) UCRM at 28 d.
Figure 10. Mechanical properties of mixtures with steel slag. (a) UCS at 7 d; (b) BS at 28 d; (c) UCRM at 28 d.
Materials 15 08277 g010aMaterials 15 08277 g010b
Figure 11. Volume stability results. (a) Treated with CH3COOH; (b) Addition of silica fume.
Figure 11. Volume stability results. (a) Treated with CH3COOH; (b) Addition of silica fume.
Materials 15 08277 g011
Figure 12. Shrinkage of mixtures with different steel slag content (4% cement content). (a) Moisture loss; (b) Shrinkage coefficient.
Figure 12. Shrinkage of mixtures with different steel slag content (4% cement content). (a) Moisture loss; (b) Shrinkage coefficient.
Materials 15 08277 g012
Figure 13. Heavy metal precipitation of different cement content.
Figure 13. Heavy metal precipitation of different cement content.
Materials 15 08277 g013
Figure 14. Heavy metal precipitation at different salinity.
Figure 14. Heavy metal precipitation at different salinity.
Materials 15 08277 g014
Figure 15. CO2eq emission of 100% limestone mixture.
Figure 15. CO2eq emission of 100% limestone mixture.
Materials 15 08277 g015
Figure 16. CO2eq emission of 50% steel slag + 50% limestone with transport distance 100 km.
Figure 16. CO2eq emission of 50% steel slag + 50% limestone with transport distance 100 km.
Materials 15 08277 g016
Figure 17. CO2eq emission of 30% steel slag + 70% limestone with transport distance 100 km.
Figure 17. CO2eq emission of 30% steel slag + 70% limestone with transport distance 100 km.
Materials 15 08277 g017
Figure 18. Detailed CO2eq emissions for each procedure.
Figure 18. Detailed CO2eq emissions for each procedure.
Materials 15 08277 g018
Table 1. Physical and mechanical properties of steel slag and limestone.
Table 1. Physical and mechanical properties of steel slag and limestone.
IndexSteel SlagLimestone
Aging 0 MonthAging 6 MonthsAging 12 Months
Apparent density (g/cm3) 4.75~9.5 mm3.5513.4823.3742.661
9.5~19 mm3.5563.4963.3872.641
19~26.5 mm3.5553.4753.3972.667
Crushing value (%) 17.418.419.225.4
Abrasion (%) 1212.51322.7
Elongated or flaky particle content (%) 4.63.93.25.3
Water absorption (%) 0.5 h1.101.081.010.29
1 h2.252.222.110.61
2 h2.452.412.300.64
4 h2.542.482.330.71
8 h2.662.602.410.72
12 h2.762.682.440.80
24 h2.962.872.530.92
48 h3.082.952.691.02
Table 2. Chemical composition of steel slag (%).
Table 2. Chemical composition of steel slag (%).
Oxide TypeCaOFe2O3SiO2MgOMnAl2O3P2O5f-CaOf-MgOOthers
Aging 0 month48.2619.0116.416.63.743.731.233.420.0371.02
Aging 6 month44.520.6217.866.433.563.541.652.430.0341.84
Aging 12 month40.7422.2319.316.263.383.352.071.440.0282.66
Table 3. OMC and MDD of different steel slag content and cement content.
Table 3. OMC and MDD of different steel slag content and cement content.
CombinationsOMC (%)MDD (g/cm3)
0% steel slag + 3% cement3.982.237
0% steel slag + 4% cement4.102.325
0% steel slag + 5% cement4.322.414
0% steel slag + 6% cement4.872.498
30% steel slag + 3% cement4.112.344
30% steel slag + 4% cement4.312.409
30% steel slag + 5% cement4.552.450
30% steel slag + 6% cement5.172.542
50% steel slag + 3% cement5.012.503
50% steel slag + 4% cement5.372.544
50% steel slag + 5% cement5.622.579
50% steel slag + 6% cement6.272.599
75% steel slag + 3% cement6.972.606
75% steel slag + 4% cement7.212.620
75% steel slag + 5% cement7.382.641
75% steel slag + 6% cement8.112.653
Table 4. Energy consumptions for unit material production [19].
Table 4. Energy consumptions for unit material production [19].
MaterialsElectricity (MJ/kg)Diesel (MJ/kg)
Cement0.36-
Limestone0.008280.000542
Steel slag--
Table 5. Cr precipitation (mg/L).
Table 5. Cr precipitation (mg/L).
Time<0.0750.075~0.60.6~2.362.36~4.754.75~9.59.5~1919~26.5
4 h7.9456.2144.9974.1033.4122.8452.217
8 h8.2136.9455.2754.8333.7893.1702.454
12 h8.5176.8435.6784.7913.6152.5762.526
16 h8.3426.7325.1614.8943.8492.7552.498
20 h8.4016.6485.5014.7973.3803.0072.505
24 h8.4436.7135.3294.9013.6672.5712.536
Table 6. V precipitation(mg/L).
Table 6. V precipitation(mg/L).
Time<0.0750.075~0.60.6~2.362.36~4.754.75~9.59.5~1919~26.5
4 h5.5624.7154.2103.7323.4892.2411.985
8 h5.7465.2134.8744.1253.8892.5152.221
12 h6.2455.6325.1874.4023.9142.6262.314
16 h6.4545.6215.2344.6983.9512.6482.369
20 h6.3545.5985.1464.5263.8792.5452.254
24 h6.215.6345.0984.3953.8812.5562.246
Table 7. Costs of material and transportation.
Table 7. Costs of material and transportation.
ItemUnit/(¥/t) *Cement-Stabilized LimestoneCement-Stabilized Limestone + 50% Steel SlagCement-Stabilized Limestone + 50% Steel
Slag + 3% Silica Fume
Cement-Stabilized Limestone + 30% Steel SlagCement-Stabilized Limestone + 30% Steel slag + 3% Silica Fume
Amount/tCost/¥Amount/tCost/¥Amount/tCost/¥Amount/tCost/¥
MaterialsCement500595297,600644321792644321,792609304,512609304,512
Limestone10014,8801,488,0007388738,8087388738,80810,1181,011,82810,1181,011,828
Steel slag10--870287,015870287,015510751,073510751,073
Water463422218993145899314568223896822389
Silica fume700----261182,732--153107,254
Transportationtkm0.35 212,486 412,491 421,628 324,675 330,038
Total - 2,000,307 1,563,252 1,755,120 1,694,477 1,807,093
Note *: The unit price is from Fangchenggang Construction Bureau in March 2022, China.
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Huang, Y.; Yang, X.; Wang, S.; Liu, Z.; Liu, L.; Xu, B. Evaluating Cement Treated Aggregate Base Containing Steel Slag: Mechanical Properties, Volume Stability and Environmental Impacts. Materials 2022, 15, 8277. https://doi.org/10.3390/ma15238277

AMA Style

Huang Y, Yang X, Wang S, Liu Z, Liu L, Xu B. Evaluating Cement Treated Aggregate Base Containing Steel Slag: Mechanical Properties, Volume Stability and Environmental Impacts. Materials. 2022; 15(23):8277. https://doi.org/10.3390/ma15238277

Chicago/Turabian Style

Huang, You, Xin Yang, Shuai Wang, Zhaohui Liu, Li Liu, and Bo Xu. 2022. "Evaluating Cement Treated Aggregate Base Containing Steel Slag: Mechanical Properties, Volume Stability and Environmental Impacts" Materials 15, no. 23: 8277. https://doi.org/10.3390/ma15238277

APA Style

Huang, Y., Yang, X., Wang, S., Liu, Z., Liu, L., & Xu, B. (2022). Evaluating Cement Treated Aggregate Base Containing Steel Slag: Mechanical Properties, Volume Stability and Environmental Impacts. Materials, 15(23), 8277. https://doi.org/10.3390/ma15238277

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop