Next Article in Journal
On Structural and Magnetic Properties of Substituted SmCo5 Materials
Next Article in Special Issue
Electroplastic Effect during Tension and Bending in Duplex Stainless Steel
Previous Article in Journal
A Study of Strength Parameter Evolution and a Statistical Damage Constitutive Model of Cemented Sand and Gravel
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Increasing the Corrosion Resistance in the UNS S32750 Super Duplex Steel Welded Joints through Hybrid GTAW-Laser Welding and Nitrogen

by
Arthur M. Videira
1,2,
Willians R. Mendes
1,
Vicente A. Ventrella
2 and
Irene Calliari
3,*
1
Department of Control and Automation Engineering, Federal Institute of Education, Science and Technology of Mato Grosso, Primavera do Leste 78850-000, Brazil
2
Department of Mechanical Engineering, São Paulo State University, Ilha Solteira 15385-000, Brazil
3
Department of Industrial Engineering, University of Padova, 35131 Padova, Italy
*
Author to whom correspondence should be addressed.
Materials 2023, 16(2), 543; https://doi.org/10.3390/ma16020543
Submission received: 8 December 2022 / Revised: 24 December 2022 / Accepted: 30 December 2022 / Published: 5 January 2023
(This article belongs to the Special Issue Advances in Duplex Stainless Steels (Second Volume))

Abstract

:
The development of techniques to improve the welding of super duplex steels is necessary in order to ensure that the phase balance and properties of the material are not affected during this process. Hybrid arc-laser welding is a perfect combination of the advantages of both processes, producing deeper weld beads with more balanced phases than the pulsed laser process. Here, the objective was to improve the corrosion resistance of UNS S32750 weld beads by increasing the volumetric austenite percentage in the fusion zone (FZ) with a hybrid process of GTAW (gas tungsten arc welding) and pulsed laser Nd-YAG (neodymium-doped yttrium aluminum garnet). Welds were performed in bead on plate conditions with fixed laser parameters and a varying heat input introduced through the GTAW process. Additionally, welds within a nitrogen atmosphere were performed. After base metal characterization, an analysis of the FZ and heat affected zone were performed with optical microscopy, scanning electron microscopy and critical pitting tests (CPT). The synergy between the thermal input provided by the hybrid process and austenite-promoting characteristic of nitrogen led to a balanced volumetric austenite/ferrite fraction. Consequently, the results obtained in CPT tests were better than conventional welding processes, such as laser or GTAW solely.

1. Introduction

Super duplex stainless steels have characteristics that combine good mechanical properties and corrosion resistance, as they consist of a two-phase structure with 50% ferrite (δ) and 50% austenite (γ) volumetric fractions. Therefore, the development of techniques to maintain the properties of super duplex steels is necessary to ensure that the phase balance and material properties are not severely impaired in this process.
The welding process leads to microstructural changes, unbalancing the phase fractions in the welded joint and surrounding areas, reducing the mechanical and corrosion resistance in these regions. Moreover, cracks may occur due to the thermal cycles involved in the welding process, with localized heating and cooling, and expansion and contraction [1]. Welding processes, such as GTAW (gas tungsten arc welding) and pulsed Nd-YAG Laser (neodymium-doped yttrium aluminum garnet), can be applied in super duplex plates, as long as welding parameters that promote phase balance are used. Previous studies showed that the use of these processes, controlling only the heat input, produce microstructures with a higher percentage of ferrite [2,3]. The reason is the very high cooling rate, avoiding the transformation of primary ferrite into austenite [4,5]. Increasing the amount of δ in the welded joint is detrimental to the corrosion resistance characteristics for several reasons.
Ferrite has lower pitting resistance equivalent numbers (PREN) than austenite, as it has lower levels of N, favoring the pitting corrosion and also promoting lower values in critical pitting temperature (CPT) tests [6,7,8].
The possible existence of depleted Cr regions due to the precipitation of Cr nitrides close to the δ grain boundaries is critical for corrosion properties as well. Furthermore, δ is rich in ferritizing elements (Cr, Mo, Si) and its formation during the welding cycle can lead to a decrease in the Cr content in adjacent metal phases, which justifies the lower corrosion resistance when there is more ferrite than austenite in the fusion zone (FZ) [6]. Another reason for ferrite to be controlled at the welded joint is that it reduces toughness at low temperatures [7].
As shown in the Cr–Ni–68%Fe pseudobinary diagram (Figure 1), the solidification of super duplex steels starts with primary ferrite, which turns into austenite [3,7,8,9]. The addition of nitrogen in the molten pool favors the formation of austenite because it acts by displacing the solvus line of the Cr–Ni–68%Fe pseudobinary diagram [10], increasing (hatched region) the biphasic area (austenite (γ) + ferrite (δ)) in Figure 1.
In other words, the addition of nitrogen in the FZ of the material provides more time for the ferrite (δ) to become austenite (γ), increasing the volumetric percentage of γ present in the weld bead.
A previous study [1] constructed the temperature profile during laser welding on a duplex steel sheet, concluding that the material cools down quickly, inhibiting the formation of austenite in the welded joint, as the FZ reaches 300 °C in less than 1 s after welding, being far from the austenite formation temperatures shown in Figure 1. In this sense, the graphs in Figure 2 demonstrate the effects of nitrogen in increasing the time for γ formation during Nd-YAG pulsed laser welding, hybrid GTAW–pulsed laser and hybrid GTAW–pulsed laser with nitrogen addition. Furthermore, the increase in heat input ensures a greater absorption of nitrogen in the FZ [12].
When comparing the graphs in Figure 2, we conclude that adding nitrogen to the hybrid GTAW pulsed laser process can be an excellent solution: with the heat input from the GTAW process, which already promotes the formation of austenite, there will be a longer time and more energy for nitrogen absorption, promoting a higher percentage of austenite in the FZ, improving its resistance to corrosion and, at the same time, obtaining a deeper penetration with the pulsed laser process.
Then, the objective was to obtain, through the hybrid GTAW (gas tungsten arc welding)/pulsed Nd-YAG (neodymium-doped yttrium aluminum garnet) laser welding process, a volumetric fraction of at least 50% austenite in the FZ and, consequently, better results in critical pitting temperature (CPT) tests than the single pulsed laser welding in the super duplex stainless steel UNS S32750.
The novelty of this work is to demonstrate the viability of hybrid GTAW laser welding to control the volumetric fraction of the ferrite/austenite phases in the FZ, revealing that it is possible to obtain balanced phases in super duplex steel sheets with a continuous welding process.

2. Materials and Methods

The base material was a UNS S32750 super duplex stainless steel sheet of 3.0 mm thickness with nominal chemical composition shown in Table 1.
The weld beads were made with a Nd-YAG pulsed laser (neodymium-doped yttrium aluminum garnet) process (LA and LN), and a hybrid GTAW (gas tungsten arc welding)/Nd-YAG pulsed laser (H20, H40, H20N and H40N) process, all in bead on plate conditions (“N” indicates samples with nitrogen addition). To perform the hybrid welding, a GTAW torch from a rectifier source was assembled with the laser turret and N2 nozzle. They worked simultaneously according to the parameters set out in Table 2. The process was automated through a holder that fixed the plate to be welded, moving it under the GTAW torch, N2 nozzle and laser aim in a linear movement at a constant and controlled speed, as shown in Figure 3a. The laser aim was focused on the surface and directed immediately after the GTAW torch, so that it shot after formation and into the GTAW molten pool in the metal, providing greater and deeper heating of the sheet and increasing N2 absorption. The working distance was 2 mm (Figure 3b).
The required conditions for the pulsed laser process were defined as the parameters that obtained an approximate depth of 1.5 mm (half the thickness of the UNS S32750 steel plate). In this way, it was possible to reach a minimum penetration for the sheet to be joined on both sides through the proposed process. These parameters were reached experimentally, controlling the frequency, temporal width and peak power, so that weld bead depths of 1.5 mm in the plate were obtained at a rate of 70% overlap. Furthermore, previous works were considered to establish the parameters of the welding processes [13,14,15,16,17]. The GTAW setup was an AWS EWTh2 tungsten electrode with 2.0 mm diameter, 45° angle, 2 mm arc length and direct current. While welding, the voltage was around 10 V and the heat input from GTAW process was considered with a 75% efficiency [18]. Table 2 shows the welding conditions for all samples.
Then, each weld bead was cut into three sections, which were metallographically prepared using sanding and polishing, providing three samples of each welding condition. The analysis of the base metal, fusion zone and heat affected zone (HAZ) was performed using optical microscopy (OM) and scanning electron microscopy (SEM), after etching these samples with Beraha’s reagent for 10 s [19]. The phase balance in volumetric fraction percentage (%V) was evaluated with the software ImageJ, with the average and standard deviation of the three sections of each condition obtained. In the same way, their geometry was measured and calculated. In sequence, the top surface of each weld bead was cleaned and protected with a heat resistant varnish, leaving a delimited area of 1 cm² exposed for critical pitting temperature (CPT) tests. Finally, the CPT tests were performed according to ASTM G150 standards [20] on the surfaces of each weld bead.

3. Results and Discussion

3.1. Base Metal

The characterization of the base metal as received was carried out by analyzing the volumetric fraction of ferrite (δ) and austenite (γ). Observations using MO and SEM revealed a volumetric fraction of each phase of around 50% and a typical microstructure of super duplex stainless steel (Table 3), consisting of a ferrite matrix with elongated austenite islands in the lamination direction (Figure 4), as obtained by previous authors [21,22]. The CPT test (Figure 5a) obtained a value of 92 °C (Figure 5b), which was compatible with the literature [23,24,25]. Thus, the base metal was in perfect condition for the proposed study.

3.2. Weld Beads

All weld beads presented a good surface finish without visual defects, but the weld beads with nitrogen addition (LN, H20N and H40N) had a lighter and brighter surface (Figure 6). In Table 4, there is a summary of the results obtained, while Figure 7 shows the cross sections of each weld bead.
Comparing the weld beads geometries, the hybrid process was able to produce joints with a higher depth when compared to the single laser process, allowing the welding of thicker plates (Table 4). The microstructure in the FZ of weld beads LA and LN was composed of primary ferrite (δ), whose orientation followed the cooling direction during welding (Figure 7). These characteristics were in accordance with the descriptions of previous authors [26,27], who claimed that in materials with a high Cr/Ni ratio the solidification in FZ firstly produces only ferrite, followed by nucleation of austenite at the grain boundaries of the already solidified ferrite, in a solid-state transformation (Figure 8a).
The pulsed laser conditions for super duplex steels are known for producing a weld bead with a low content of austenite [2] and a FZ microstructure based on a ferritic matrix and much less austenite than the base metal. In addition, Figure 8b (LA) shows intragranular austenite bands due to overlapping laser pulses, which provided more energy for their nucleation inside the grains [28]. The heat input and the short time of the laser pulse did not keep the material at the required temperature for long enough for the large scale transformation of ferrite to austenite. Some regions of the FZ did not even show visible austenite grains in OM (Figure 9a). Comparing LA and LN conditions (Table 4), there was no significant difference in the austenite %V results, because in the LN condition, the short laser pulse time and the low heat input were not sufficient to allow the N2 to interact with the welding pool. Thus, in all the weld beads formed with pulsed laser only, the %V of austenite, considering also specific regions of the FZ, varied from 0.01 to 8%, which corroborated findings from previous studies that showed a decrease in austenite %V in the FZ in processes with low heat inputs and fast cooling rates [13,14,15,16,17].
In Figure 9b the HAZ was very small, being imperceptible, and it was not possible to delimit it. Therefore, we confirmed that the pulsed Nd-YAG laser welding on UNS S32750 steel produced unbalanced joints. The high volumetric fraction of ferrite found in the FZ (Table 4 and Figure 7) can be detrimental to corrosion resistance and may have caused the poor performance in CPT tests, where a lower content of austenite in the FZ resulted in lower CPT values of around 26 °C for LA and 27 °C for LN.
In another way, when applying the hybrid process in the H20 and H40 conditions, the heat input from GTAW provided more energy to the solid-state transformation of ferrite to austenite, increasing the austenite %V in the FZ, as shown in Table 4 and Figure 10 (H20 and H40). In the H20N and H40N conditions, the N2 flow directed to the metal molten pool resulted in a higher %V in the FZ (Figure 10) because the GTAW welding pool provided more time and a higher energy for the nitrogen to penetrate in the FZ [12], while the laser shots allowed the nitrogen to penetrate deeper into the weld bead, as shown in Figure 7, where each laser pulse in the H20N condition left one deeper austenite layer in the section. This phenomenon is clear to see when comparing the H20N and H40N conditions: increasing the GTAW current in the weld bead (Figure 10) produced a high content of austenite, reaching around 50% of each phase.
As in the LA and LN conditions, the microstructure morphology in the FZ of hybrid weld beads showed epitaxial growth of the grains in the cooling direction (Figure 7, Figure 8 and Figure 9). The morphology of austenite present in the hybrid weld’s FZ (Figure 10) was also characteristic of intergranular and intragranular nucleation, but it also had some regions with austenite growth occurring in plates, known as Widmanstatten γ. The latter does not form at lower heat inputs, such as those found in LA and LN weld beads, because it needs more energy, as it results from the detachment of austenite plates previously formed in the grain boundaries (intergranular γ) [13,28,29,30].
The results of the CPT tests were improved with the hybrid welding (Figure 11) due to the increase in the %V of austenite in the FZ, reaching 37 °C (H20) and 45 °C (H40). With the addition of N2 in hybrid welding, values of 67 °C (H20N) and 74 °C (H40N) were obtained for the same reason. Thus, N2 and an increased thermal input promoted better results in the CPT tests.
In brief, when compared to the pulsed laser or GTAW processes [2,31,32], all hybrid welds with nitrogen addition presented a higher volumetric fraction of austenite in the FZ, resulting in a good corrosion resistance, reaching higher values (74 °C in the H40N) than the pulsed laser welding (Figure 11). The hybrid welding with N2 addition proved to be effective to promote the interaction of the N2 with the fusion pool, increasing the austenite %V in the fusion zone, reaching more than 50%, and improving the corrosion resistance of the joint.

4. Conclusions

The low heat input of pulsed laser welding did not allow primary ferrite to transform into austenite. Furthermore, the energy was not sufficient for nitrogen to interact with the welding pool, meaning that its addition was not effective. Consequently, the pulsed laser conditions analyzed produced weld beads with a low content of austenite, impairing the corrosion resistance and achieving low values in the CPT tests.
In comparison to the pulsed laser welding process with the same parameters, the greater heat input of the GTAW process, which keeps the metal temperature in the range of austenite formation for longer, resulted in a higher volumetric percentage of austenite when applying the GTAW pulsed laser welding in UNS S32750. Furthermore, the hybrid joints corrosion resistance was improved through hybrid welding, as shown in the CPT test results. The hybrid process allowed the nitrogen to interact with the welding pool and proved that nitrogen addition can be beneficial to the fusion zone, increasing the austenite volumetric fraction and corrosion resistance, and achieving a better performance in the CPT tests. Moreover, the hybrid welding promoted deeper fusion zone penetration, producing deeper weld beads when compared to using GTAW or pulsed laser only. The morphology of austenite present in the FZ of all weld beads was characteristic of intergranular and intragranular nucleation, but in the hybrid welding the presence of Widmanstatten γ was noticed due the higher heat input.
The results showed an innovative manufacturing process with known parameters providing excellent corrosion properties in the welded beads. The correct adjustment of welding conditions can promote a high production rate in industry, as the welded joints could be produced with the desired properties without the need for subsequent heat treatments.
For future works, we suggest obtaining the elemental composition of the FZ. This could be useful to verify the amount of nitrogen absorbed. Moreover, performing hybrid welding beads with an increase in the heat input above that used in this work would allow thicker plates to be welded.

Author Contributions

Conceptualization, A.M.V. and V.A.V.; methodology, A.M.V. and V.A.V.; validation, A.M.V., W.R.M., V.A.V. and I.C.; formal analysis, A.M.V., W.R.M., V.A.V. and I.C.; investigation, A.M.V.; resources, V.A.V. and I.C.; data curation, A.M.V. and V.A.V.; writing—original draft preparation, A.M.V.; writing—review and editing, A.M.V., W.R.M., V.A.V. and I.C.; visualization, A.M.V. and W.R.M.; supervision, V.A.V. and I.C.; project administration, V.A.V. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding.

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Zambon, A.; Bonollo, F. Rapid solidification in laser welding of stainless steels. Mater. Sci. Eng. A 1994, 178, 203–207. [Google Scholar] [CrossRef]
  2. da Cruz Junior, E.J.; Franzini, O.D.; Calliari, I.; Ventrella, V.A. Effects of Nickel Addition on the Microstructure of Laser-Welded UNS S32750 Duplex Stainless Steel. Metall. Mater. Trans. A 2019, 50, 1616–1618. [Google Scholar] [CrossRef]
  3. Zhang, Z.; Jing, H.; Xu, L.; Han, Y.; Zhao, L.; Zhou, C. Effects of nitrogen in shielding gas on microstructure evolution and localized corrosion behavior of duplex stainless steel welding joint. Appl. Surf. Sci. 2017, 404, 110–128. [Google Scholar] [CrossRef]
  4. Eghlimi, A.; Shamanian, M.; Eskandarian, M.; Zabolian, A.; Nezakat, M.; Szpunar, J.A. Evaluation of microstructure and texture across the welded interface of super duplex stainless steel and high strength low alloy steel. Surf. Coat. Technol. 2015, 264, 150–162. [Google Scholar] [CrossRef]
  5. Eghlimi, A.; Shamanian, M.; Eskandarian, M.; Zabolian, A.; Szpunar, J.A. Characterization of microstructure and texture across dissimilar super duplex/austenitic stainless steel weldment joint by super duplex filler metal. Mater. Charact. 2015, 106, 27–35. [Google Scholar] [CrossRef]
  6. Köse, C.; Topal, C. Texture, microstructure and mechanical properties of laser beam welded AISI 2507 super duplex stainless steel. Mater. Chem. Phys. 2022, 289, 126490. [Google Scholar] [CrossRef]
  7. Nithin Raj, P.; Sivan, A.P.; Sekar, K.; Joseph, M.A. Effect of Austenite Reformation on Localized Corrosion Resistance of Hyper-Duplex Stainless Steel in Hot Chloride Solution. Inter. J. Metalcast. 2020, 14, 167–178. [Google Scholar] [CrossRef]
  8. Ma, C.Y.; Zhou, L.; Zhang, R.X.; Li, D.G.; Shu, F.Y.; Song, X.G.; Zhao, Y.Q. Enhancement in mechanical properties and corrosion resistance of 2507 duplex stainless steel via friction stir processing. J. Mater. Res. Technol. 2020, 9, 8296–8305. [Google Scholar] [CrossRef]
  9. Maftoum, R.A.; Borges, P.C.; Marqueze, C.M. Influência do nitrogênio na resistência à erosão por cavitação do aço inoxídavel martensítico. Matéria 2017, 22, e11933. [Google Scholar] [CrossRef] [Green Version]
  10. Lundin, C.D.; Russel, S.W. The Development of Qualification Standards for Cast Duplex Stainless Steel; Materials Joining Group—Materials Science and Engineering, University of Tennessee Knoxville: Knoxville, TN, USA, 2005; p. 166. [Google Scholar]
  11. Ramírez-Londoño, A.J. Precipitação das Fases Intermetálicas e Austenita Secundária na ZAC de Soldagens Multipasse de Aços Inoxidáveis Duplex; Tese (Doutorado em Engenharia Metalúrgica e de Materiais)—Escola Politécnica da Universidade de São Paulo: São Paulo, Brazil, 2001; p. 241. [Google Scholar]
  12. Reyes-Hernández, D.; Manzano-Ramírez, A.; Encinas, A.; Sánchez-Cabrera, V.M.; Marroquín De Jesús, Á.; García-García, R.; Orozco, G.; Olivares-Ramírez, J.M. Addition of nitrogen to GTAW welding duplex steel 2205 and its effect on fatigue strength and corrosion. Fuel 2017, 198, 165–169. [Google Scholar] [CrossRef]
  13. Videira, A.M.; Crespo, G.S.; Ventrella, V.A. Application of pulsed laser Nd:YAG in superduplex steel UNS S 32750: Autogenous laser welding, Laser welding with refusion process by laser and Hybrid welding (laser/GTAW). In Nd:YAG Lasers: Technology and Applications; Larry, P.T., Ed.; Nova Science Publishers: New York, NY, USA, 2020; Volume 1, pp. 63–89. [Google Scholar]
  14. Kangda, H.; Chen, Z.; Xiaoyan, Z.; Ming, G. Effect of heat input on weld microstructure and toughness of laser-arc hybrid welding of martensitic stainless steel. J. Mater. Process. Technol. 2017, 245, 7–14. [Google Scholar]
  15. Ramkumar, K.D.; Mishra, D.; Raj, B.G.; Vignesh, M.K.; Thiruvengatam, G.; Sudharshan, S.P.; Arivazhagan, N.; Sivashanmugam, N.; Rabel, A.M. Effect of optimal weld parameters in the microstructure and mechanical properties of autogeneous gas tungsten arc weldments of super-duplex stainless steel UNS S32750. Mater. Des. 2015, 66, 356–365. [Google Scholar] [CrossRef]
  16. Jagesvar, V.; Ravindra, V.T. Effect of welding processes and conditions on the microstructure, mechanical properties and corrosion resistance of duplex stainless steel weldments—A review. J. Manuf. Process. 2017, 25, 134–152. [Google Scholar]
  17. Saravanan, S.; Raghukandan, K.; Sivagurumanikandan, N. Pulsed Nd: YAG laser welding and subsequent post-weld heat treatment on super duplex stainless steel. J. Manuf. Process. 2017, 25, 284–289. [Google Scholar] [CrossRef]
  18. Jafarzadegan, M.; Taghiabadi, R.; Mofid, M.A. Using double ellipsoid heat source model for prediction of HAZ grain growth in GTAW of stainless steel 304. Mater. Today Commun. 2022, 31, 103411. [Google Scholar] [CrossRef]
  19. ASTM E407-07 e1; Standard Practice for Microetching Metals and Alloys. ASTM International: West Conshohocken, PA, USA, 2015.
  20. ASTM G150; Standard Test Method for Electrochemical Critical Pitting Temperature Testing of Stainless Steels. Mai: Philadelphia, PA, USA, 2013.
  21. Maurya, A.K.; Pandey, C.; Chhibber, R. Effect of filler metal composition on microstructural and mechanical characterization of dissimilar welded joint of nitronic steel and super duplex stainless steel. Arch. Civ. Mech. Eng. 2022, 22, 1–28. [Google Scholar] [CrossRef]
  22. Rodrigues, D.G.; Braga Maria, G.G.; Viana, N.A.L.; Santos, D.B. Effect of low cold-rolling strain on microstructure, texture, phase transformation, and mechanical properties of 2304 lean duplex stainless steel. Mater. Charact. 2019, 150, 138–149. [Google Scholar] [CrossRef]
  23. Zhao, K.; Li, X.Q.; Wang, L.W.; Yang, Q.R.; Cheng, L.J.; Cui, Z.Y. Passivation Behavior of 2507 Super Duplex Stainless Steel in Hot Concentrated Seawater: Influence of Temperature and Seawater Concentration. Acta Metall. Sin. (Engl. Lett.) 2022, 35, 326–340. [Google Scholar] [CrossRef]
  24. Guo, Y.; Liang, P.; Shi, Y.; Zhao, Y.; Li, F.; Jin, L. Effect of Hydrogen on Corrosion Behavior of S32750 Super Duplex Stainless Steel. Int. J. Eletrochem. Sci. 2018, 13, 10302–10313. [Google Scholar] [CrossRef]
  25. Gennari, C.; Lago, M.; Bögre, B.; Mészáros, I.; Calliari, I.; Pezzato, L. Microstructural and Corrosion Properties of Cold Rolled Laser Welded UNS S32750 Duplex Stainless Steel. Metals 2018, 8, 1074. [Google Scholar] [CrossRef] [Green Version]
  26. Mohammed, G.R.; Ishak, M.; Agida, S.N.; Abdulhadi, H.A. Effects of heat input on microstructure, corrosion and mechanical characteristics of welded austenitic and duplex stainless steel: A review. Metals 2017, 7, 39. [Google Scholar] [CrossRef] [Green Version]
  27. Mohammed, G.R.; Ishak, M.; Agida, S.N.; Abdulhadi, H.A. Fiber laser welding of dissimilar 2205/304 stainless steel plates. Metals 2017, 7, 546. [Google Scholar] [CrossRef]
  28. Magalhães CH, X.M.; Faria GL, D.; Lagoeiro, L.E.; Silva, J.D. Characterization of the Austenite Reformation Mechanisms as a Function of the Initial Ferritic State in a UNS S32304 Duplex Stainless Steel. Mater. Res. 2017, 20, 1470–1479. [Google Scholar] [CrossRef] [Green Version]
  29. Varbai, B.; Pickle, T.; Májlinger, K. Effect of heat input and role of nitrogen on the phase evolution of 2205 duplex stainless steel weldment. Int. J. Press. Vessel. Pip. 2019, 176, 103952. [Google Scholar] [CrossRef]
  30. Fonseca, C.S.; Pinheiro, I.P.; Silva, S.N. Influência do aporte térmico sobre a morfologia da austenita e na quantidade das fases em chapas soldadas de aço inoxidável duplex SAF2205. Matéria 2016, 21, 227–234. [Google Scholar] [CrossRef]
  31. Videira, A.M. Influência do aporte térmico da soldagem GTAW no balanço de fases Ferrita/Austenita do Aço Inoxidável Duplex UNS S32205; Dissertação (Mestrado em Engenharia Mecânica)—São Paulo State University: São Paulo, Brazil, 2016; p. 98. Available online: http://hdl.handle.net/11449/136319 (accessed on 25 October 2022).
  32. Videira, A.M. Soldagem híbrida GTAW-Laser Nd-YAG Pulsado: Efeitos no Aço Inoxidável Superduplex UNS S32750; Tese (Doutorado em Engenharia Mecânica)—São Paulo State University: São Paulo, Brazil, 2022; p. 139. Available online: http://hdl.handle.net/11449/202840 (accessed on 27 October 2022).
Figure 1. Cr–Ni–68%Fe pseudobinary diagram adapted by the authors [11]. The addition of N2 expands the biphasic δ + γ field.
Figure 1. Cr–Ni–68%Fe pseudobinary diagram adapted by the authors [11]. The addition of N2 expands the biphasic δ + γ field.
Materials 16 00543 g001
Figure 2. Time (t) the fusion zone remains in biphasic zone (δ + γ) while cooling in (a) pulsed laser Nd-YAG welding, (b) hybrid GTAW pulsed laser welding and (c) hybrid GTAW pulsed laser welding with nitrogen addition.
Figure 2. Time (t) the fusion zone remains in biphasic zone (δ + γ) while cooling in (a) pulsed laser Nd-YAG welding, (b) hybrid GTAW pulsed laser welding and (c) hybrid GTAW pulsed laser welding with nitrogen addition.
Materials 16 00543 g002
Figure 3. (a) Hybrid GTAW laser welding arrangement. (b) Laser camera view.
Figure 3. (a) Hybrid GTAW laser welding arrangement. (b) Laser camera view.
Materials 16 00543 g003
Figure 4. SEM pictures of the base material as received. (a) Reveals a balanced austenite/ferrite microstructure, with elongated geometry due to the lamination process; (b) Detail of austenite in high relief and ferrite in low relief due to Beraha etching.
Figure 4. SEM pictures of the base material as received. (a) Reveals a balanced austenite/ferrite microstructure, with elongated geometry due to the lamination process; (b) Detail of austenite in high relief and ferrite in low relief due to Beraha etching.
Materials 16 00543 g004
Figure 5. (a) Base metal surface after the CPT test. Arrows indicate pitting corrosion. (b) CPT test graph of the base metal, showing the current reaching 100 μA at a temperature of 92 °C.
Figure 5. (a) Base metal surface after the CPT test. Arrows indicate pitting corrosion. (b) CPT test graph of the base metal, showing the current reaching 100 μA at a temperature of 92 °C.
Materials 16 00543 g005
Figure 6. Top view of the weld beads. No visual defects found.
Figure 6. Top view of the weld beads. No visual defects found.
Materials 16 00543 g006
Figure 7. OM of weld bead cross sections. The %V of austenite in FZ increased from samples LA to H40N due to higher values of heat input and nitrogen addition.
Figure 7. OM of weld bead cross sections. The %V of austenite in FZ increased from samples LA to H40N due to higher values of heat input and nitrogen addition.
Materials 16 00543 g007
Figure 8. OM of LA weld bead showing (a) intergranular γ and (b) the effect of laser overlap on γ dispersion.
Figure 8. OM of LA weld bead showing (a) intergranular γ and (b) the effect of laser overlap on γ dispersion.
Materials 16 00543 g008
Figure 9. OM of LN weld bead where (a) the γ is imperceptible and (b) there is an undefined HAZ.
Figure 9. OM of LN weld bead where (a) the γ is imperceptible and (b) there is an undefined HAZ.
Materials 16 00543 g009
Figure 10. OM of weld bead sections H20, H40, H20N and H40N. The %V of austenite in FZ increased with higher values of heat input and nitrogen addition.
Figure 10. OM of weld bead sections H20, H40, H20N and H40N. The %V of austenite in FZ increased with higher values of heat input and nitrogen addition.
Materials 16 00543 g010
Figure 11. Graph with CPT test curves from each weld bead and base metal, showing the current reaching 100 μA.
Figure 11. Graph with CPT test curves from each weld bead and base metal, showing the current reaching 100 μA.
Materials 16 00543 g011
Table 1. Chemical composition of UNS S32750 super duplex steel.
Table 1. Chemical composition of UNS S32750 super duplex steel.
Composition (%)CCrCuMoMnNNiPSSi
Max0.03026.00.55.01.20.328.00.0350.020.8
Min-24.0-3.0-0.246.0---
Table 2. Welding parameters.
Table 2. Welding parameters.
Weld BeadWelding Speed (mm/s)Pulsed Laser ParametersGTAW ParameterTotal Heat Input (J/mm)Gas Flow Rate (L/min)
Frequency (Hz)Peak Energy (kW)Time Width (ms)Current (A)ArN2
LA262.510-75150
LN262.510-75018
H20262.51020150150
H40262.51040225150
H20N262.510201501518
H40N262.510402251518
Table 3. Base metal phase balance.
Table 3. Base metal phase balance.
Austenite (%V)Ferrite (%V)Standard DeviationCPT (°C)
49.950.1±0.392
Table 4. Weld bead phase balance in percentage of volumetric fraction (%V); geometry obtained, with all values followed by the standard deviation (±); and CPT results.
Table 4. Weld bead phase balance in percentage of volumetric fraction (%V); geometry obtained, with all values followed by the standard deviation (±); and CPT results.
Weld BeadAustenite (%V)Depth (mm)Width (mm)CPT (°C)
LA7.3 ± 1.01.75 ± 0.031.38 ± 0.0426
LN7.5 ± 2.11.74 ± 0.041.40 ± 0.0127
H2011.1 ± 2.62.06 ± 0.061.86 ± 0.0337
H4015.8 ± 1.32.60 ± 0.042.85 ± 0.0445
H20N34.4 ± 12.02.10 ± 0.022.03 ± 0.0267
H40N51.3 ± 7.72.67 ± 0.023.54 ± 0.0574
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.

Share and Cite

MDPI and ACS Style

Videira, A.M.; Mendes, W.R.; Ventrella, V.A.; Calliari, I. Increasing the Corrosion Resistance in the UNS S32750 Super Duplex Steel Welded Joints through Hybrid GTAW-Laser Welding and Nitrogen. Materials 2023, 16, 543. https://doi.org/10.3390/ma16020543

AMA Style

Videira AM, Mendes WR, Ventrella VA, Calliari I. Increasing the Corrosion Resistance in the UNS S32750 Super Duplex Steel Welded Joints through Hybrid GTAW-Laser Welding and Nitrogen. Materials. 2023; 16(2):543. https://doi.org/10.3390/ma16020543

Chicago/Turabian Style

Videira, Arthur M., Willians R. Mendes, Vicente A. Ventrella, and Irene Calliari. 2023. "Increasing the Corrosion Resistance in the UNS S32750 Super Duplex Steel Welded Joints through Hybrid GTAW-Laser Welding and Nitrogen" Materials 16, no. 2: 543. https://doi.org/10.3390/ma16020543

APA Style

Videira, A. M., Mendes, W. R., Ventrella, V. A., & Calliari, I. (2023). Increasing the Corrosion Resistance in the UNS S32750 Super Duplex Steel Welded Joints through Hybrid GTAW-Laser Welding and Nitrogen. Materials, 16(2), 543. https://doi.org/10.3390/ma16020543

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.