Optimization of Processing Steps for Superior Functional Properties of (Ba, Ca)(Zr, Ti)O3 Ceramics
Next Article in Special Issue
Surface Analysis of Ti-Alloy Micro-Grooved 12/14 Tapers Assembled to Non-Sleeved and Sleeved Ceramic Heads: A Comparative Study of Retrieved Hip Prostheses
Previous Article in Journal
Fabrication of SiCN(O) Aerogel Composites with Low Thermal Conductivity by Wrapping Mesoporous Aerogel Structures over Mullite Fibers
Previous Article in Special Issue
Nanotopography Evaluation of NiTi Alloy Exposed to Artificial Saliva and Different Mouthwashes
 
 
Font Type:
Arial Georgia Verdana
Font Size:
Aa Aa Aa
Line Spacing:
Column Width:
Background:
Article

Influence of Tantalum Addition on the Corrosion Passivation of Titanium-Zirconium Alloy in Simulated Body Fluid

by
El-Sayed M. Sherif
1,*,
Yassir A. Bahri
2,
Hamad F. Alharbi
2,
Muhammad Farzik Ijaz
2 and
Ibrahim A. Alnaser
1,2
1
Centre of Excellence for Research in Engineering Materials (CEREM), King Saud University, P.O. Box 800, Riyadh 11421, Saudi Arabia
2
Mechanical Engineering Department, Collage of Engineering, King Saud University, P.O. Box 800, Riyadh 11421, Saudi Arabia
*
Author to whom correspondence should be addressed.
Materials 2022, 15(24), 8812; https://doi.org/10.3390/ma15248812
Submission received: 22 November 2022 / Revised: 7 December 2022 / Accepted: 8 December 2022 / Published: 9 December 2022
(This article belongs to the Special Issue Corrosion of Metals for Biomedical Applications)

Abstract

:
Ti-15%Zr alloy and Ti-15%Zr-2%Ta alloy were fabricated to be used in biomedical applications. The corrosion of these two alloys after being immersed in simulated body fluid for 1 h and 72 h was investigated. Different electrochemical methods, including polarization, impedance, and chronoamperometric current with time at 400 mV were employed. Also, the surface morphology and the compositions of its formed film were reported by the use of scanning electron microscope and energy dispersive X-ray. Based on the collected results, the presence of 2%Ta in the Ti-Zr alloy passivated its corrosion by minimizing its corrosion rate. The polarization curves revealed that adding Ta within the alloy increases the corrosion resistance as was confirmed by the impedance spectroscopy and current time data. The change of current versus time proved that the addition of Ta reduces the absolute current even at high anodic potential, 400 mV. The results of both electrochemical and spectroscopic methods indicated that pitting corrosion does not occur for both Ti-Zr and Ti-Zr-Ta alloys, even after their immersion in SBF solutions for 72 h.

1. Introduction

The current demand for biomedical implants has shaped the need for high-quality materials to meet such a market. Statistically, it is estimated that approximately 1.0 million people undergo hip replacements annually, which further establishes the significant use of biomedical equipment on a global scale [1,2,3,4,5,6,7]. Ti-base alloys have been employing in automotive, aerospace, and biomedical employments for their excellent mechanical strength, high corrosion resistance, and good biocompatibility [4,6]. Some of the Ti-based alloys still present several mechanical performance challenges [7]. In addition, even though titanium is well known for its biocompatibility, Ti–6Al–4V is the most employed alloy for biomedical applications. This alloy contains aluminum as well as vanadium, which raises worries that ions from these metals could have a negative effect on the application [8]. It has been claimed [9,10] that Ti-6Al-4V alloy causes toxic reactions within the human body as a result of releasing of Al+3 and V+5 as free radicals, which interact with the bloodstream. This release of these cations leads to a possible risk of Alzheimer’s disease within the patients [11,12]. Because of this, it is desirable to substitute these metals for other alloying elements.
Zirconium (Zr) and tantalum (Ta) have been proposed as more stable non-toxic titanium alloys and biocompatible alternatives to these metals [13,14,15]. Zr has excellent mechanical properties, as well as a remarkable corrosion resistance, which makes it a prefect substance for biomedical implants. In addition, Ta is non-reactive with bodily fluids and is utilized in the production of surgical instruments. In addition, Ta is likewise non-irritating to the body, and it is utilized in the manufacture of surgical sutures and implants such as prosthetic joints and cranial plates, among other things. A protective oxide film formed on the outer surface of such alloys gives it excellent in-vivo performance. The formation of this layer reduces the number of the released cations into the biological medium and aids in the osseointegration process. Given that the implant surface is the only location in which living tissues come into contact, the properties of the surface coating are of particular importance [16]. It is possible to improve the resistance to corrosion and biocompatibility of permanent implant materials by altering their surface properties. Due to the excellent wear resistance of Zr, commercially available Zr knee implants with surface oxide coatings thicknesses ranging from 2–5 µm are used [17].
This study investigated the effect of adding 2% Ta on the passivation of corrosion of Ti-15Zr alloy in the simulated body fluid (SBF) solution. The SBF was selected since its effect on Ti-Zr alloy is similar to that of blood. Various techniques to evaluate the corrosion; these are the cyclic polarization, impedance, and the change of current vs. time were used for alloys after their exposure for 1 h and 72 h in the SBF solution. Scanning electron microspectroscopy and X-ray spectroscopy investigations were also conducted on the surface of the corroded samples.

2. Materials and Methods

The powders of Ti (99.9 purity and 5–7 μm particle size), Zr (99% purity and 10 μm particle size), and Ta (99.9% purity and 10 μm particle size) were supplied by Nanochemazone, Canada. Ally powders were mixed (in weight percentage) in a high-energy ball mill. To ensure the homogenous distribution for all powders, the mixing rate was 150 rpm for 30 min. The electrolyte was a simulated body fluid (SBF, Gibco® by Life technologies, New Delhi, India), which is a mixture of the following chemical substances, NaCl, KCl, Na2SO4, NaHCO3, K2HPO4, MgCl2.6H2O, and CaCl2 [18]. The manufacturing of the Ti-Zr alloy and Ti-Zr-Ta alloy was carried out with the same reported procedures in the previous study [19].
A three electrodes electrochemical cell that widen for 150 mL SBF was employed. A computer-controlled Autolab Potentiostat/Galvanostat (purchased from Metrohm, Amsterdam, The Netherlands) was utilized. The preparation of the working electrodes, which were the fabricated alloys, was carried out as in the published work [17,19]. Also, the reference and counter electrodes were the same ones that were used in the reported study [19]. The polarization curves were obtained by scanning the potential from −1000 to +400 mV at a scan rate of 2.0 mV/s. The impedance measurement experiments were collected from the corrosion potential within a frequency range between 100,000 Hz and 0.10 Hz and the data were fitted using the ZSimpWin v3.1 software [20,21,22]. The chronoamperometric current-time curves were obtained after stepping the potential at an anodic value in the SBF solution for 60 min of the actual measurement from applying the anodic constant potential, 400 mV. All experiments were performed at room temperature after 1 h and 72 h exposure to the test solution. The surface morphology was taken using a JEOL microscopy model JSM-7400F (SEM, Tokyo, Japan) and the EDX analyses were also investigated using an attached unit to the microscope.

3. Results and Discussion

3.1. Potentiodynamic Cyclic Polarization (PCP) Data

The PCP experiments were conducted to determine the effects of Ta additions on the corrosion behavior of the Ti-Zr alloy in the SBF solution at two exposure periods of time. Figure 1 presents the PCP plots for (a) Ti-Zr alloy and (b) Ti-Zr-Ta alloy after being immersed in the SBF solution for 1 h. Same procedures were also carried out after 72 h immersion and the curves of the PCP are displayed in Figure 2. The values predicted from those polarization figures are registered in Table 1. These symbols are the cathodic (βc) and anodic (βa) Tafel slopes, respectively. The corrosion potential (ECorr), the corrosion current (jCorr), the polarization resistance (RP), and the corrosion rate (RCorr). The βc, βa, jCorr and ECorr values were obtained from the plotted curves as has been reported in the earlier work [20,21,22]. The RP values as well as the RCorr values were calculated using the following relations, respectively [23,24,25,26,27]:
R P = 1 j C o r r   ( β c · β a 2.3 ( β c + β a ) )  
R C o r r = j C o r r ( k · E W d · A )
Here, k = 3272 mm (amp−1 cm−1 year−1), EW = equivalent weight, d is the density, and A is the area. Figure 1 and Figure 2 illustrated that the cathodic current tends to decrease towards the minimum value (where, jCorr and ECorr are calculated) as a result of the oxygen reduction reaction as per these reactions [27,28,29];
2H2O + O2 + 4e = 4OH
1 2 O + H 2 O + 2 e = 2 O H
For Ti-15Zr alloy and Ti-15Zr-2Ta alloy, the anodic reaction begins with increasing the current values with potential scan in the positive direction. It is also observed that the Ti-15Zr’s anodic current is higher than that of Ti-15Zr-2Ta’s anodic current at the same potential value. This means that Ti-15Zr-2Ta alloy has higher resistance to corrosion than that the Ti-15Zr alloy has. Scanning the potential in the backward direction, both Ti-15Zr alloy and Ti-15Zr-2Ta alloy provided lower current values than those obtained from the forward direction. The disappearance of hysteresis loops with both alloys indicates that the pitting attack does not occur at this condition. As the immersion period is prolonged to 72 h (Figure 2), the obtained PCP curves were similar to those recorded after only 1 h exposure (Figure 1), but with lower jCorr and ECorr values. These results are corroborated by the values recorded in Table 1, where RCorr and jCorr are smaller, whereas RP is higher for the Ti-15Zr-2Ta alloy, and this effect occurs with increasing exposure time to 72 h. Therefore, the PCP results confirm that adding 2%Ta to Ti-15Zr increases its corrosion resistance when exposed to SBF, and that this effect increases with increased exposure time. In fact, it is more than likely that the formations of TiO2, ZrO2 and TaO2 mixed oxides account for higher resistance to corrosion as well as less corrosion rates in Ti-15Zr-2Ta alloys. Meanwhile, due to the formation of TiO2 and ZrO2 in case of the Ti-15Zr alloy, it records a lower RP value and higher RCorr value than those for Ti-15Zr-2Ta alloy.

3.2. Electrochemical Impedance Spectroscopy (EIS) Measurements

The data obtained from EIS provide an explanation for the reactions of the electron transfer at the interface for the alloys and SBF solution. EIS technique has been successfully employed for reporting the corrosion and passivation phenomena under various circumstances [26,27]. Exposure to SBF solution for 1.0 h, the Nyquist plots for (a) Ti-15Zr alloy and (b) Ti-15Zr-2Ta alloy are presented in Figure 3. In addition, similar plots were also collected after 72 h at the same condition, and the spectra are depicted in Figure 4. These data were best fitted to the circuit that is displayed in Figure 5. This circuit have different impedance elements. Here, the solution resistance (RS), two different constant phase elements (Q1 and Q2), and two polarization resistances (RP1 and RP2). Table 2 presents these elements and summarizes the values of the EIS elements. In order to make sure the chosen circuit that was used here, other studies have reported the same circuit for other materials [30,31,32].
It has been proposed that the existence of CPEs in the capacitive circuit enables us to estimate the deviations from ideality. Here, Q1 with n values varying from 0.75 to 0.86 exemplify double layer capacitors with some pores to reduce the chare of the alloys’ surfaces. Furthermore, Q2 represents another double layer capacitor for its n values in the range from 0.61 and 1.0, which increases the concept that the passivation of the tested alloys in SBF solution is achieved, while the dissolution is not favorable. Also, RP1 signifies that polarization resistance exists between the surface Ti-Zr alloy and Ti-Zr-Ta alloy and the layer formed on their surfaces. Additionally, RP2 refers to the resistance at the interface between the alloys’ formed surface layer and electrolyte.
The EIS spectra of Figure 3 and Figure 4 along with the listed elements in Table 2 show that Ta rises the Ti-Zr-Ta alloy’s resistance to corrosion. This is indicated by the diameter of the obtained semicircle that is much wider than the one of the circle of Ti-Zr alloy. This was also enhanced via the higher values of the obtained polarization resistance, RP1 and RP2, as represented in Table 2. Another proof of the increase of corrosion resistance was predicted from the values of YQ1 and YQ2 as it decreases in the presence of Ta. Immersion for 72 h also has a great impact on enhancing the values of the resistance to corrosion for both Ti-Zr alloy and Ti-Zr-Ta alloy. This was revealed by increasing the diameter of the Nyquist plot (Figure 4) and the higher RP1 and RP2 values, in addition to the lower YQ1 and YQ2 values (Table 2).
Bode plots of (a) impedance of the interface (|Z|) and (b) degree of the phase angle (Φ) for (1) Ti-Zr alloy and (2) Ti-Zr-Ta alloy that were exposed to SBF for 1 h are presented in Figure 6. Similar plots were also taken for these alloys after their immersion in SBF for 72 h, as seen in Figure 7. As seen from Figure 6, the presence of Ta enhances |Z| values, and the highest value of Φ, particularly at the low frequency region. This indicates that the passivity of the Ti-Zr alloy when Ta is present increased. As compared to the values of |Z| and Φ after 1 h immersion, the plots of Figure 7 indicate that extending the time of exposure to 72 h further increases both |Z| and the highest heights of Φ, which is clearer at the low frequency values. The high corrosion resistances of both Ti-Zr and Ti-Zr-Ta alloys increase remarkably with expanded exposure time to SBF solution. The EIS results along with the PCP data confirm that adding 2% Ta greatly improves the Ti-Zr alloy’s resistance to corrosion, and this is remarkably enhanced at the longer immersion period.
Bode plots of the (a) impedance of the interface (|Z|) and (b) degree of the phase angle (Φ) for Ti-Zr alloy (1) and Ti-Zr-Ta alloy (2) after being exposed to SBF for 1 h are presented in Figure 6. The same plots were also taken for these alloys after their immersion in SBF for 72 h, as seen in Figure 7. As seen from Figure 6, the presence of Ta enhances |Z| and the highest Φ values, particularly at the low frequency region. This indicates that the passivity of the alloy when Ta is present increased. As compared to the values of |Z| and Φ after 1 h immersion, the plots of Figure 7 indicate that extending the time of exposure to 72 h further increases both |Z| and Φ, which is clearer at the low frequency values. The high corrosion resistances of both Ti-Zr and Ti-Zr-Ta alloys increase remarkably with the exposure time to SBF solution. The EIS results along with the PCP data confirm that adding 2% Ta greatly improves the Ti-Zr alloy’s resistance to corrosion and this is enhanced remarkably at the longer immersion period.

3.3. Chronoamperometric Current-Time (CCT) Measurements

The CCT plots at 400 mV were collected to report the influence of Ta on the resistance to corrosion of Ti-Zr. In particular, pitting corrosion occurs, where the CCT technique has been widely employed to report similar cases [33,34,35,36]. Figure 8 depicts the curves of the current variations vs. time of (1) Ti-Zr alloy and (2) Ti-Zr-Ta alloy over (a) 1 h and (b) 72 h in SBF, respectively. Here, the current of Ti –Zr alloy (curve 1) shows the highest values at the first moments measurement, whether the alloy is exposed for 1.0 h or 72 h. In this case, the lessening of current results from the formation of oxide film, which gives the surface an immunity against the attack of the corrosive SBF solution. Expanding the time of the potential application for ≥20 min produced a slight decrease of the current that in turn stabilizes the formed oxide layer to passivate the surface [18]. This again provides another confirmation that pitting corrosion does not take place for the alloy and general corrosion is at its minimum. The lower current values in the presence of Ta do not only passivate the surface and enhance its resistance to general corrosion but also decrease the severity of pitting corrosion. It is worth noting that expanding the time to 72 h leads to an increase in corrosion resistance.

3.4. SEM and EDX Analyses

The effect of adding 2% Ta on the surface morphology of Ti-Zr alloy after being immersed in SBF for 3 days and stepping a 400 mV as a constant anodic potential for an hour was determined by scanning electron microscope (SEM) images. Figure 9 shows the SEM image and the energy dispersive X-ray (EDX) spectra for Ti-15Zr under the aforementioned conditions. The SEM image of Figure 9 displays that the Ti-15Zr alloy surface does not show any deep pits with the possibility of formation of some corrosion products. The chemical components found on that surface for the Ti-15Zr sample that is shown in the EDX were only Ti, Zr, and O, with proportional weights of 64.19% (Ti), 22.05% (O), and 13.7% (Zr) respectively, and atomic of 46.67% (Ti), 45.86% (O), and 7.47% (Zr). According to the collected results, the detected O content indicates that the formed surface film on the alloy probably is a mixture of TiO2 and ZrO2, and thus the passivation of Ti-Zr alloy in SBF solution is increased, and pitting corrosion is prevented from taking place [19].
Figure 10 displays (a) SEM and (b) EDX analyses for Ti-15Zr-2Ta alloy that were taken under the same procedures considered for Ti-15Zr alloy. It is clear that the surface of Ti-15Zr-2Ta alloy is more similar to the surface of Ti-15Zr and that no clear pittings appear. The EDX spectrum confirmed the presence in weight % of 66.53% Ti, 14.99% Zr, 1.56% Ta, and 16.91% O, which is equivalent to the atomic % of 53.03% Ti, 6.27% Zr, 0.33% Ta, and 40.36% O, on the surface of the Ti-Zr-Ta alloy. The presence of high oxygen content again suggests a thick oxide layer that consists of TiO2, ZrO2, and TaO2 is formed on the surface. The surface morphology using SEM and the elemental analysis using EDX tools are thus consistent with the electrochemical data, which proved the influence of 2% Ta addition, namely that it remarkably increases the resistance to corrosion of the titanium alloy. As compared to the reported research on pure Ti [19], CP-Ti [37], TaC nanocrystalline coating [38], Ti-7.5%Mo [39], and also compared to our previous works on Ti-6%Alalloy, Ti-6%Al-4%V alloy [35], and Ti-6Al-xV alloys [36], the fabricated Ti-Zr-Ta here has low corrosion rate and excellent corrosion resistance. Moreover, compared to the Zhou et al. [5] who reported the corrosion resistance, wear resistance, and biocompatibility of Ti-10Ta alloy, Ti-30Ta alloy, and Ti-70Ta alloy, the presence of Zr and Ta within Ti in our tested Ti-Zr and Ti-Zr-Ta alloys has greatly improved the corrosion resistance.

4. Conclusions

The passivation of corrosion of Ti-15%Zr alloy and Ti-15%Zr-2%Ta alloy, which were fabricated from their milled powders using HFHIF, after being immersed for in SBF solution 1 h and 72 h, were investigated. The PCP results indicated that the addition of 2% Ta decreased the corrosion of Ti-15Zr alloy by decreasing its corrosion current and thus its corrosion rate, which increases its corrosion resistance. EIS Nyquist and Bode plots also confirmed that the presence of 2% Ta minimizes corrosion of Ti-15Zr alloy through increasing the diameter of the obtained semicircle and the values of the impedance of the interface as well as the maximum of the degree of the phase angle. By comparing Ti-15%Zr-2%Ta alloy with Ti-15%Zr, CCT measurements demonstrated that the absolute currents were lower when Ta was present in the alloy. The increase of time of immersion for the tested alloys in SBF solution has been found to reduce their corrosion via the thickening of a mixture of oxide layers. The surface investigations confirmed that Ta passivates the corrosion of Ti-Zr alloy via the formation of TiO2, ZrO2 and TaO2. All results support the proposal that the investigated alloys can provide a great benefit in employment in biomedical applications. Compared to the other reported pure Ti and Ti-base alloys; i.e., Ti-6Al, Ti-6Al-2V, Ti-6Al-4V, Ti-6Al-6V, Ti-6Al-8V, the manufactured Ti-Zr and Ti-Zr-Ta alloys produce lower corrosion rate and higher corrosion resistance.

Author Contributions

Conceptualization, E.-S.M.S., Y.A.B. and H.F.A.; methodology, E.-S.M.S. and Y.A.B.; software, E.-S.M.S., Y.A.B. and H.F.A.; validation, E.-S.M.S., Y.A.B., H.F.A., M.F.I. and I.A.A.; formal analysis, E.-S.M.S. and Y.A.B.; investigation, E.-S.M.S. and Y.A.B.; resources, E.-S.M.S. and Y.A.B.; data curation, E.-S.M.S., Y.A.B., H.F.A., M.F.I. and I.A.A.; writing—original draft preparation, E.-S.M.S. and Y.A.B.; writing—review and editing, E.-S.M.S.; visualization, E.-S.M.S., Y.A.B., H.F.A., M.F.I. and I.A.A.; supervision, E.-S.M.S. and H.F.A.; project administration, E.-S.M.S. and H.F.A.; funding acquisition, E.-S.M.S. All authors have read and agreed to the published version of the manuscript.

Funding

This work was financially supported by the Deputyship for Research & Innovation, Ministry of Education in Saudi Arabia through the project no. (IFKSURG-2-1150).

Institutional Review Board Statement

Not applicable.

Informed Consent Statement

Not applicable.

Data Availability Statement

Not applicable.

Acknowledgments

The authors extend their appreciation to the Deputyship for Research & Innovation, Ministry of Education in Saudi Arabia for funding this research work through the project no. (IFKSURG-2-1150).

Conflicts of Interest

The authors declare no conflict of interest.

References

  1. Chicardi, E.; García-Garrido, C.; Sayagués, M.; Torres, Y.; Amigó, V.; Aguilar, C. Development of a novel fcc structure for an amorphous-nanocrystalline Ti-33Nb-4Mn (at.%) ternary alloy. Mater. Charact. 2018, 135, 46–56. [Google Scholar] [CrossRef]
  2. Yu, Z. Titanium Alloys for Biomedical Development and Applications. In Design, Microstrcature, Properties, and Application; Elsevier Inc.: Amsterdam, The Netherlands, 2022; eBook; ISBN1 9780128241653. Paperback; ISBN2 9780128239278. [Google Scholar] [CrossRef]
  3. Boyer, R.R. An overview on the use of titanium in the aerospace industry. Mater. Sci. Eng. A 1996, 213, 103–114. [Google Scholar] [CrossRef]
  4. Geetha, M.; Singh, A.K.; Muraleedharan, K.; Gogia, A.K.; Asokamani, R. Effect of thermomechanical processing on microstructure of a Ti-13Nb-13Zr alloy. J. Alloys Compd. 2001, 329, 214–223. [Google Scholar] [CrossRef]
  5. Zhou, Y.L.; Niinomi, M.; Akahori, T.; Fukui, H.; Toda, H. Corrosion resistance and biocompatibility of Ti–Ta alloys for biomedical applications. Mater. Sci. Eng. A. 2005, 398, 28–36. [Google Scholar] [CrossRef]
  6. Hao, Y.L.; Yang, R.; Niinomi, M.; Kuroda, D.; Zhou, Y.L.; Fukunaga, K.; Suzuki, A. Young modulus and mechanical properties of Ti–29Nb–13Ta– 4.6Zr in relation to α” martensite”. Metallug. Mater. Trans. A 2002, 33, 3137–3144. [Google Scholar] [CrossRef]
  7. Zohdy, K.M.; El-Sherif, R.M.; El-Shamy, A.M. Corrosion and Passivation Behaviors of Tin in Aqueous Solutions of Different pH. J. Bio-Tribo-Corros. 2021, 7, 74. [Google Scholar] [CrossRef]
  8. Tkachenko, S.; Datskevich, O.; Kulak, L.; Jacobson, S.; Engqvist, H.; Persson, C. Wear and friction properties of experimental Ti–Si–Zr alloys for biomedical applications. J. Mech. Behav. Biomed. Mater. 2014, 39, 61–72. [Google Scholar] [CrossRef]
  9. Li, R.; Liu, G.; Yang, L.; Qing, Y.A.; Tang, X.; Guo, D.; Zhang, K.; Qin, Y. Tantalum boride as a biocompatible coating to improve osteogenesis of the bionano interface. J. Biomed. Mater. Res. A 2020, 108, 1726–1735. [Google Scholar] [CrossRef]
  10. Li, Y.; Yang, C.; Zhao, H.; Qu, S.; Li, X.; Li, Y. New developments of Ti-based alloys for biomedical applications. Materials 2014, 7, 1709–1800. [Google Scholar] [CrossRef]
  11. Kawahara, M.; Kato-Negishi, M. Link between Aluminum and the Pathogenesis of Alzheimer’s Disease: The Integration of the Aluminum and Amyloid Cascade Hypotheses. Int. J. Alzheimer’s Dis. 2011, 2011, 276393; [Google Scholar] [CrossRef] [Green Version]
  12. Kandimalla, R.; Vallamkondu, J.; Corigat, E.B.; Gill, K.D. Understanding Aspects of Aluminum Exposure in Alzheimer’s Disease Development. Brain Pathol. 2016, 26, 139–154. [Google Scholar] [CrossRef] [PubMed]
  13. Grandin, H.M.; Berner, S.; Dard, M. A review of titanium zirconium (TiZr) alloys for use in endosseous dental implants. Materials 2012, 5, 1348–1360. [Google Scholar] [CrossRef] [Green Version]
  14. Biehl, V.; Wack, T.; Winter, S.; Seyfert, U.T.; Breme, J. Evaluation of the hemocompatibility of titanium-based biomaterials. Biomol. Eng. 2002, 19, 97–101. [Google Scholar] [CrossRef] [PubMed]
  15. Chong, Y.; Bhattacharjee, T.; Tsuji, N. Bi-lamellar microstructure in Ti–6Al–4V: Microstructure evolution and mechanical properties. Mater. Sci. Eng. A. 2019, 762, 138077. [Google Scholar] [CrossRef]
  16. Sanchez, A.G.; Schreiner, W.; Duffó, G.U.S.T.A.V.O.; Ceré, S.I.L.V.I.A. Surface characterization of anodized zirconium for biomedical applications. Appl. Surf. Sci. 2011, 257, 6397–6405. [Google Scholar] [CrossRef]
  17. Abdel-Hady, M.; Fuwa, H.; Hinoshita, K.; Kimura, H.; Shinzato, Y.; Morinaga, M. Phase stabilities change with Zr content in β-type Ti–Nb alloys. Scr. Mater. 2007, 57, 1000–1003. [Google Scholar] [CrossRef]
  18. Khalil, K.A.; Sherif, E.-S.M.; Almajid, A.A. Corrosion passivation in Simulated Body Fluid of Magnesium/Hydroxyapatite Nanocomposites Sintered by High Frequency Induction Heating. Int. J. Electrochem. Sci. 2011, 6, 6184–6199. [Google Scholar]
  19. Alharbi, H.F.; Bahri, Y.A.; Sherif, E.-S.M. Influence of Zirconium on the Corrosion Passivation of Titanium in Simulated Body Fluid. Crystals 2021, 11, 1391. [Google Scholar] [CrossRef]
  20. Sherif, E.-S.M.; Erasmus, R.M.; Comins, J.D. In situ Raman spectroscopy and electrochemical techniques for studying corrosion and corrosion inhibition of iron in sodium chloride solutions. Electrochim. Acta 2010, 55, 3657–3663. [Google Scholar] [CrossRef]
  21. Sherif, E.-S.M. Effects of 5-(3-aminophenyl)-tetrazole on the inhibition of unalloyed iron corrosion in aerated 3.5% sodium chloride solutions as a corrosion inhibitor. Mater. Chem. Phys. 2011, 129, 961–967. [Google Scholar] [CrossRef]
  22. Sherif, E.-S.M. Corrosion and corrosion inhibition of pure iron in neutral chloride solutions by 1,1’-thiocarbonyldiimidazole. Int. J. Electrochem. Sci. 2011, 6, 3077–3092. [Google Scholar]
  23. AlOtaibi, A.; Sherif, E.-S.M.; Zinelis, S.; Al Jabbari, Y.S. Corrosion Behavior of Two cp Titanium Dental Implants Connected by Cobalt Chromium Metal Superstructure in Artificial Saliva and the Influence of Immersion Time. Int. J. Electrochem. Sci. 2016, 11, 5877–5890. [Google Scholar] [CrossRef]
  24. Sherif, E.-S.M. Corrosion Behavior of Duplex Stainless Steel Alloy Cathodically Modified with Minor Ruthenium Additions in Concentrated Sulfuric Acid Solutions. Int. J. Electrochem. Sci. 2011, 6, 2284–2298. [Google Scholar]
  25. Sherif, E.S.M. Effects of exposure time on the anodic dissolution of Monel-400 in aerated stagnant sodium chloride solutions. J. Solid State Electrochem. 2012, 16, 891–899. [Google Scholar] [CrossRef]
  26. Sherif, E.-S.M.; Ahmed, A.H.; Abdo, H.S.; DefAllah, M.N. Impediment of Iron Corrosion by N,N’-bis [2-hydroxynaphthylidene] amino]oxamide in 3.5% NaCl solution. Crystals 2021, 11, 1263. [Google Scholar] [CrossRef]
  27. Sherif, E.S.M.; Potgieter, J.H.; Comins, J.D.; Cornish, L.; Olubambi, P.A.; Machio, C.N. The beneficial effect of ruthenium additions on the passivation of duplex stainless-steel corrosion in sodium chloride solutions. Corros. Sci. 2009, 51, 1364–1371. [Google Scholar] [CrossRef]
  28. Sherif, E.-S.M.; Ahmed, A.H. Alleviation of Iron Corrosion in Chloride Solution by N,N0-bis [2-Methoxynaphthylidene]amino]oxamide as a Corrosion Inhibitor. Crystals 2021, 11, 1516. [Google Scholar] [CrossRef]
  29. Badawy, W.A.; Al-Kharafi, F.M.; El-Azab, A.S. Electrochemical behaviour and corrosion inhibition of Al, Al-6061 and Al-Cu in neutral aqueous solutions. Corros. Sci. 1999, 41, 709–727. [Google Scholar] [CrossRef]
  30. Gopi, D.; Sherif, E.-S.M.; Manivannan, V.; Rajeswari, D.; Surendiran, M.; Kavitha, L. Corrosion and Corrosion Inhibition of Mild Steel in Groundwater at Different Temperatures by Newly Synthesized Benzotriazole and Phosphono Derivatives. Ind. Eng. Chem. Res. 2014, 53, 4286–4294. [Google Scholar] [CrossRef]
  31. Sherif, E.-S.M.; Abdo, H.S.; Almajid, A.A. Corrosion Behavior of Cast Iron in Freely Aerated Stagnant Arabian Gulf Seawater. Materials 2015, 8, 2127–2138. [Google Scholar] [CrossRef] [Green Version]
  32. Afzali, P.; Ghomashchi, R.; Oskouei, R.H. On the corrosion Behaviour of low modulus titanium alloys for medical implant applications: A review. Metals 2019, 9, 878. [Google Scholar] [CrossRef] [Green Version]
  33. Latief, F.; Sherif, E.-S.M.; Almajid, A.; Junaedi, H. Fabrication of exfoliated graphite nanoplatelets-reinforced aluminum composites and evaluating their mechanical properties and corrosion behavior. J. Anal. Appl. Pyrolysis 2011, 92, 485–492. [Google Scholar] [CrossRef]
  34. Sherif, E.-S.M.; Park, S.-M. Effects of 1,5-Naphthalenediol on Aluminum Corrosion as a Corrosion Inhibitor in 0.50 M NaCl. J. Electrochem. Soc. 2005, 152, B205–B211. [Google Scholar] [CrossRef] [Green Version]
  35. Sherif, E.-S.M.; Ragab, S.A.; Abdo, H.S. Role of Vanadium Additions on the Corrosion Mitigation of Ti-6Al-xV Alloy in Simulated Body Fluid. Metals 2020, 10, 903. [Google Scholar] [CrossRef]
  36. Abdo, H.S.; Sherif, E.-S.M.; El-Serehy, H.A. Manufacturing of Ti-6%Al and Ti-6%Al-4%V Alloys and Their Corrosion in Sodium Chloride Solutions. Crystals 2020, 10, 181. [Google Scholar] [CrossRef] [Green Version]
  37. Arslan, E.; Totik, Y.; Demirci, E.; Alsaran, A. Influence of surface roughness on corrosion and tribological behavior of CP-Ti after thermal oxidation treatment. J. Mater. Eng. Perform. 2009, 19, 428–433. [Google Scholar] [CrossRef]
  38. Zhao, Y.; Xu, J.; Peng, S. Synthesis and evaluation of TaC nanocrystalline coating with excellent wear resistance, corrosion resistance, and biocompatibility. Ceramics Inter. 2021, 47, 20032–20044. [Google Scholar] [CrossRef]
  39. Hsu, H.-C.; Wu, S.-C.; Hsu, S.-K.; Chang, T.-Y.; Ho, W.-F. Effect of ball milling on properties of porous Ti–7.5Mo alloy for biomedical applications. J. Alloys Compud. 2014, 582, 793–801. [Google Scholar] [CrossRef]
Figure 1. PCP curves of (a) Ti-Zr alloy and (b) Ti-Zr-Ta alloy immersed in SBF for 1.0 h.
Figure 1. PCP curves of (a) Ti-Zr alloy and (b) Ti-Zr-Ta alloy immersed in SBF for 1.0 h.
Materials 15 08812 g001
Figure 2. PCP curves of (a) Ti-Zr alloy and (b) Ti-Zr-Ta alloy immersed in SBF for 72 h.
Figure 2. PCP curves of (a) Ti-Zr alloy and (b) Ti-Zr-Ta alloy immersed in SBF for 72 h.
Materials 15 08812 g002
Figure 3. Nyquist plots for (a) Ti-Zr alloy and (b) Ti-Zr-Ta alloy after their immersion in SBF solution for 1.0 h.
Figure 3. Nyquist plots for (a) Ti-Zr alloy and (b) Ti-Zr-Ta alloy after their immersion in SBF solution for 1.0 h.
Materials 15 08812 g003
Figure 4. Nyquist plots for (a) Ti-Zr alloy and (b) Ti-Zr-Ta alloy after their immersion in SBF solution for 72 h.
Figure 4. Nyquist plots for (a) Ti-Zr alloy and (b) Ti-Zr-Ta alloy after their immersion in SBF solution for 72 h.
Materials 15 08812 g004
Figure 5. The R(QR(QR)) equivalent circuit model.
Figure 5. The R(QR(QR)) equivalent circuit model.
Materials 15 08812 g005
Figure 6. (a) Bode |Z| and (b) Bode Φ plots for (1) Ti-Zr alloy and (2) Ti-Zr-Ta alloy that were immersed in SBF for 1 h.
Figure 6. (a) Bode |Z| and (b) Bode Φ plots for (1) Ti-Zr alloy and (2) Ti-Zr-Ta alloy that were immersed in SBF for 1 h.
Materials 15 08812 g006
Figure 7. (a) Bode |Z| and (b) Bode Φ plots for (1) Ti-Zr alloy and (2) Ti-Zr-Ta alloy that were immersed in SBF for 72 h.
Figure 7. (a) Bode |Z| and (b) Bode Φ plots for (1) Ti-Zr alloy and (2) Ti-Zr-Ta alloy that were immersed in SBF for 72 h.
Materials 15 08812 g007
Figure 8. The CCT plots for (1) Ti-Zr alloy and (2) Ti-Zr-Ta alloy after (a) 1 h and (b) 72 h exposure to SBF solution, the applied potential was 400 mV, respectively.
Figure 8. The CCT plots for (1) Ti-Zr alloy and (2) Ti-Zr-Ta alloy after (a) 1 h and (b) 72 h exposure to SBF solution, the applied potential was 400 mV, respectively.
Materials 15 08812 g008
Figure 9. The SEM and EDX for Ti-Zr alloy after its exposure for 3 days in SBF before stepping the potential to 400 mV.
Figure 9. The SEM and EDX for Ti-Zr alloy after its exposure for 3 days in SBF before stepping the potential to 400 mV.
Materials 15 08812 g009
Figure 10. The SEM and EDX for Ti-Zr-Ta alloy after its exposure for 3 days in SBF before stepping the potential to 400 mV.
Figure 10. The SEM and EDX for Ti-Zr-Ta alloy after its exposure for 3 days in SBF before stepping the potential to 400 mV.
Materials 15 08812 g010
Table 1. Parameters estimated from the PCP curves.
Table 1. Parameters estimated from the PCP curves.
Alloyβc (V dec−1)ECorr (V)βa (V dec−1)jCorr (mA/cm2)RP (kΩ cm2)RCorr (mmy−1)
Ti−Zr (1.0 h)1901604250.5568.666.40 × 10−3
Ti−Zr-Ta (1.0 h)1401503650.3589.964.09 × 10−3
Ti−Zr (72 h)1601803150.4581.845.23 × 10−3
Ti−Zr-Ta (72 h)1501703000.30115.493.49 × 10−3
Table 2. EIS parameters represented in Figure 5.
Table 2. EIS parameters represented in Figure 5.
AlloyRS/Ω cm2Q1RP1/Ω cm2Q2RP2/Ω cm2
YQ1/F cm−2nYQ2/F cm−2n
Ti−Zr (1.0 h)60.30.04180.7843600.00931.005512
Ti−Zr-Ta (1.0 h)72.40.04110.8668690.00660.618400
Ti−Zr (72 h)62.50.03190.8010,1220.00510.8120,653
Ti−Zr-Ta (72 h)122.50.02120.7512,5260.00120.9026,850
Publisher’s Note: MDPI stays neutral with regard to jurisdictional claims in published maps and institutional affiliations.

Share and Cite

MDPI and ACS Style

Sherif, E.-S.M.; Bahri, Y.A.; Alharbi, H.F.; Ijaz, M.F.; Alnaser, I.A. Influence of Tantalum Addition on the Corrosion Passivation of Titanium-Zirconium Alloy in Simulated Body Fluid. Materials 2022, 15, 8812. https://doi.org/10.3390/ma15248812

AMA Style

Sherif E-SM, Bahri YA, Alharbi HF, Ijaz MF, Alnaser IA. Influence of Tantalum Addition on the Corrosion Passivation of Titanium-Zirconium Alloy in Simulated Body Fluid. Materials. 2022; 15(24):8812. https://doi.org/10.3390/ma15248812

Chicago/Turabian Style

Sherif, El-Sayed M., Yassir A. Bahri, Hamad F. Alharbi, Muhammad Farzik Ijaz, and Ibrahim A. Alnaser. 2022. "Influence of Tantalum Addition on the Corrosion Passivation of Titanium-Zirconium Alloy in Simulated Body Fluid" Materials 15, no. 24: 8812. https://doi.org/10.3390/ma15248812

APA Style

Sherif, E. -S. M., Bahri, Y. A., Alharbi, H. F., Ijaz, M. F., & Alnaser, I. A. (2022). Influence of Tantalum Addition on the Corrosion Passivation of Titanium-Zirconium Alloy in Simulated Body Fluid. Materials, 15(24), 8812. https://doi.org/10.3390/ma15248812

Note that from the first issue of 2016, this journal uses article numbers instead of page numbers. See further details here.

Article Metrics

Back to TopTop